Find suppliers for this alloyC67600
Chemical Composition
Element
Cu(1,2)PbSnZnFeMn
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min.
Min (%)57.00.500.500.400.05
Max (%)60.01.01.5Rem1.30.50
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Section Size
(in)
Rod1/2 HardH0284   Typ
60   Typ
19   Min
90   Typ
1
1/4 HardH0172   Typ
42   Typ
27   Min
77   Typ
2
H0177   Typ
45   Typ
23   Min
83   Typ
1
Soft AnnealO6065   Typ
30   Typ
33   Min
65   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1630
Melting Point - Solidus°F1590
Densitylb/cu in. at 68°F0.302
Electrical Conductivity% IACS at 68°F24
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F61
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.8
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingFair
Spot WeldGood
Capacity for Being Cold WorkedPoor
Capacity for Being Hot FormedExcellent
Forgeability Rating80
Machinability Rating60
Fabrication Process Properties

No fabrication process properties for this alloy

Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
IndustrialGate Valve StemsCorrosion ResistanceCorrosion Resistance
Gate Valve StemsMachining CharacteristicsMachinability
Gate Valve StemsMechanical PropertiesHigh Strength
Valve BallsCorrosion ResistanceCorrosion Resistance
Valve BallsFriction & Wear PropertiesWear Resistance
Valve BallsMachining CharacteristicsMachinability
Welding RodConductivity (Electrical)Electrical Conductivity
Welding RodCorrosion ResistanceOxidation Resistance
Applicable Specifications
Form Sub-Form System Standard Description
Brazing Filler MetalAWSA5.8BRAZING FILLER METAL
Die ForgingHot-PressedASTMB138/B138MMANGANESE BRONZE ROD, BAR AND SHAPES
Forgings, Die (Hot Pressed)ASMESB283COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
ASTMB283/B283MCOPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
Rod, Bar & ShapesASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
Corrosion Properties

No information available.