Find suppliers for this alloy
C69100
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | Ni | Al | Mn | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||||||||
| Min (%) | 81.0 | 0.8 | 0.7 | 0.8 | |||||
| Max (%) | 84.0 | 0.05 | 0.10 | Rem | 0.25 | 1.4 | 1.2 | 0.10 | 1.3 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Section Size (in) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| Tube | Cast and Annealed (homogenized) | O10 |
70 Typ |
35 Typ |
45 Typ |
72 Typ |
37 Typ |
0.022 |
| Melting Point - Liquidus°F | 2012 |
|---|---|
| Melting Point - Solidus°F | 1846 |
| Densitylb/cu in. at 68°F | 0.308 |
| Specific Gravity | 8.53 |
| Electrical Conductivity% IACS at 68°F | 15 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 10.6 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 10.6 |
| Modulus of Elasticity in Tensionksi | 16900 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Not Recommended |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Not Recommended |
| Forgeability Rating | 55 |
| Machinability Rating | 78 |
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Tube, hydraulic and pneumatic | Forming Characteristics | Formability |
| Tube, hydraulic and pneumatic | Magnetic Properties | Non-Magnetic | |
| Tube, hydraulic and pneumatic | Mechanical Properties | Cryogenic Properties | |
| Tube, hydraulic and pneumatic | Solderability | Solderability |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Pipe | ASTM | B706 | SEAMLESS COPPER ALLOY (UNS NO. C69100) PIPE AND TUBE | ||
| Seamless Pipe and Tube | C69100 Alloy | ASME | SB706 | SEAMLESS PIPE AND TUBE | |
| Tube | ASTM | B706 | SEAMLESS COPPER ALLOY (UNS NO. C69100) PIPE AND TUBE |
Corrosion Properties