Find suppliers for this alloyC69410
Chemical Composition
Element
Cu(1)PbZnFeSi
(1) Cu + Sum of Named Elements 99.5% min.
Min (%)8111.03.5
Max (%)0.0915.00.204.5
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Section Size
(in)
Forgings1/8 HardH00100   Typ
57   Typ
21   Typ
95   Typ
0.75
RodSoft AnnealO6080   Typ
40   Typ
25   Typ
85   Typ
2.0
O6085   Typ
43   Typ
25   Typ
85   Typ
1.0
O6090   Typ
45   Typ
20   Typ
85   Typ
0.5
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1685
Melting Point - Solidus°F1510
Densitylb/cu in. at 68°F0.296
Specific Gravity8.19
Electrical Conductivity% IACS at 68°F6.2
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F15
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.2
Modulus of Elasticity in Tensionksi16000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingGood
Spot WeldGood
Seam WeldGood
Butt WeldGood
Capacity for Being Cold WorkedPoor
Capacity for Being Hot FormedExcellent
Forgeability Rating80
Machinability Rating30
Fabrication Process Properties

No fabrication process properties for this alloy

Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
PlumbingLead-free,dezincification resistant alloy for potable water components
Low Lead Valves and Fittings
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.