C69750
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P | Ni(3) | Mn | Si | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. (3) Ni value includes Co. |
|||||||||
| Min (%) | 78.0 | 0.8 | 1.9 | ||||||
| Max (%) | 83.0 | 1.3 | 0.05 | Rem | 0.05 | 0.02 | 0.01 | 0.05 | 2.22 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 3000 gm | Section Size (in) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| Rod | Soft Anneal | O60 |
65 Min 68 Typ |
22 Min 36 Typ |
50 Typ |
105 Min |
>.020 |
| Spring | H08 |
102 Min 109 Typ |
87 Min 94 Typ |
8 Typ |
200 Min |
>.475 | |
| Spring | H08 |
131 Min 138 Typ |
116 Min 119 Typ |
1 Typ |
260 Min |
<.315 | |
| Spring | H08 |
109 Min 116 Typ |
94 Min 102 Typ |
5 Typ |
220 Min |
<.475 | |
| Wire | Soft Anneal | O60 |
65 Min 68 Typ |
22 Min 36 Typ |
50 Typ |
105 Min |
>.020 |
| Spring | H08 |
102 Min 109 Typ |
87 Min 94 Typ |
8 Typ |
200 Min |
>.475 | |
| Spring | H08 |
131 Min 138 Typ |
116 Min 119 Typ |
1 Typ |
260 Min |
<.315 | |
| Spring | H08 |
109 Min 116 Typ |
94 Min 102 Typ |
5 Typ |
220 Min |
<.475 | |
| Melting Point - Liquidus°F | 1724 |
|---|---|
| Melting Point - Solidus°F | 1562 |
| Densitylb/cu in. at 68°F | 0.311 |
| Specific Gravity | 8.6 |
| Electrical Conductivity% IACS at 68°F | 9.5 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 23 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 11.1 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.091 |
| Modulus of Elasticity in Tensionksi | 15200 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Fair |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Good |
| Seam Weld | Excellent |
| Butt Weld | Excellent |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 30 |
| Machinability Rating | 90 |
Common Fabrication Processes
| Treatment | Minimum* | Value* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Stress Relief | 590 | |||
| Annealing | 1020 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Electrical Connectors | Conductivity (Electrical) | Electrical Conductivity |
| Electrical Connectors | Forming Characteristics | Formability | |
| Electrical Pinions | Conductivity (Electrical) | Electrical Conductivity | |
| Electrical Pinions | Forming Characteristics | Formability | |
| Electronic Contacts | Conductivity (Electrical) | Electrical Conductivity | |
| Electronic Contacts | Forming Characteristics | Formability |
Applicable Specifications
Corrosion Properties