Find suppliers for this alloy
C70315
Elements | ||||||||||
---|---|---|---|---|---|---|---|---|---|---|
Cu(1) | Pb | Sn | Zn | Fe | P | Ni | Ag | Mg | Si | |
(1) Cu + Sum of Named Elements 99.5% min. |
||||||||||
Min (%) | 1.0 | 0.08 | ||||||||
Max (%) | Rem | 0.05 | 1.0 | 2.0 | 0.10 | 0.05 | 4.0 | 0.50 | 0.20 | 1.0 |
Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 3000 gm |
---|---|---|---|---|---|---|
* Measured at room temperature, 68°F (20°C). | ||||||
Strip, Sheet, Rod, Bar | 1/2 Hard | H02 |
67 Min 75 Max |
60 Min |
7 Typ |
135 Min 165 Max |
1/4 Hard | H01 |
60 Min 68 Max |
52 Min |
9 Typ |
125 Min 155 Max |
|
1/8 Hard | H00 |
52 Min 62 Max |
36 Min |
14 Typ |
100 Min 130 Max |
|
3/4 Hard | H03 |
75 Min 84 Max |
67 Min |
5 Typ |
145 Min 175 Max |
|
Extra Hard | H06 |
84 Min 94 Max |
75 Min |
4 Typ |
170 Min 200 Max |
|
Mill-hardened Temper, TM - 1/2 Hard | TM02 |
96 Min 109 Max |
86 Min |
10 Typ |
200 Min 250 Max |
|
Mill-hardened Temper, TM - 1/2 Hard | TM01 |
90 Min 104 Max |
78 Min |
16 Typ |
180 Min 240 Max |
|
Mill-hardened Temper, TM - Hard | TM04 |
109 Min 120 Max |
99 Min |
8 Typ |
210 Min 260 Max |
|
Mill-hardened Temper, TM - SHM | TM05 |
116 Min |
109 Min |
5 Typ |
210 Min |
Melting Point - Liquidus°F | 1940 |
---|---|
Melting Point - Solidus°F | 1904 |
Densitylb/cu in. at 68°F | 0.32 |
Specific Gravity | 8.86 |
Electrical Conductivity% IACS at 68°F | 43 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 107 |
Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.5 |
Modulus of Elasticity in Tensionksi | 19100 |
Technique | Suitability |
---|---|
Soldering | Good |
Brazing | Good |
Oxyacetylene Welding | Not Recommended |
Gas Shielded Arc Welding | Good |
Coated Metal Arc Welding | Not Recommended |
Spot Weld | Fair |
Seam Weld | Fair |
Butt Weld | Fair |
Capacity for Being Cold Worked | Good |
Capacity for Being Hot Formed | Excellent |
Common Fabrication Processes
Thermal Properties
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Automotive | Electrical Connectors - Automotive | ||
Electrical | Connector Components |
Applicable Specifications
Corrosion Properties