C70340
| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1) | Sn | Zn | P | Ni | Co | Cr | Si | |
|
(1) Cu + Sum of Named Elements, 99.92% min. |
||||||||
| Min (%) | 0.05 | 1.5 | 0.20 | 0.05 | 0.40 | |||
| Max (%) | Rem | 0.50 | 0.50 | 2.5 | 0.6 | 0.15 | 0.8 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 3000 gm |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Strip | Hard | H04 |
112 Min 117 Typ 120 Max |
106 Min 113 Typ 117 Max |
4.0 Typ |
245 Typ |
| Melting Point - Liquidus°F | 1985 |
|---|---|
| Melting Point - Solidus°F | 1964 |
| Densitylb/cu in. at 68°F | 0.319 |
| Specific Gravity | 8.83 |
| Electrical Conductivity% IACS at 68°F | 50 |
| Electrical Resistivityohm.cmil/ft at 68°F | 20.742 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 121.36 |
| Modulus of Elasticity in Tensionksi | 18130 |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
Common Fabrication Processes
Typical Uses
Applicable Specifications
Corrosion Properties