Find suppliers for this alloy
C70350
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Zn | Fe | Ni | Co | Mg | Mn | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||||||||
| Min (%) | 1.0 | 1.0 | 0.50 | ||||||
| Max (%) | Rem | 0.05 | 1.0 | 0.20 | 2.5 | 2.0 | 0.15 | 0.20 | 1.2 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Flat Products | Mill-hardened Temper, TM - 1/2 Hard | TM02 |
110 Typ |
100 Typ |
6 Min |
| Mill-hardened Temper, TM - Hard | TM04 |
120 Typ |
110 Typ |
4 Min |
|
| Mill-hardened Temper, TM -XHM - Extra Hard | TM06 |
130 Typ |
120 Typ |
2 Min |
|
| Sheet | Mill-hardened Temper - SHMS | TM10 |
135 Typ |
130 Typ |
|
| Mill-hardened Temper, TM - XHMS Spring | TM08 |
145 Typ |
140 Typ |
||
| Melting Point - Liquidus°F | 2007 |
|---|---|
| Melting Point - Solidus°F | 1967 |
| Densitylb/cu in. at 68°F | 0.318 |
| Specific Gravity | 8.81 |
| Electrical Conductivity% IACS at 68°F | 50 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 115 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Modulus of Elasticity in Tensionksi | 19000 |
| Modulus of Rigidityksi | 7300 |
| Magnetic Permeability | 1.01 |
| Poisson's Ratio | 0.34 |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Spot Weld | Fair |
| Seam Weld | Fair |
| Butt Weld | Fair |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
| Forgeability Rating | 70 |
| Machinability Rating | 20 |
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Electrical Springs | ||
| Electronic Connectors |
Applicable Specifications
Corrosion Properties