| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Zn | Fe | Ni(3) | Mn | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. (3) Ni value includes Co. |
||||||
| Min (%) | 1.3 | 4.8 | 0.30 | |||
| Max (%) | Rem | 0.05 | 1.0 | 1.7 | 6.2 | 0.8 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale |
|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||||
| Strip | 1/2 Hard | H02 |
57 Typ |
55 Typ |
11 Typ |
67 Typ |
65 Typ |
||
| 1/4 Hard | H01 |
51 Typ |
40 Typ |
21 Typ |
54 Typ |
57 Typ |
|||
| Annealed | O61 |
38 Typ |
12 Typ |
41 Typ |
8 Typ |
||||
| Extra Hard | H06 |
70 Typ |
69 Typ |
3 Typ |
75 Typ |
69 Typ |
|||
| Hard | H04 |
64 Typ |
63 Typ |
5 Typ |
72 Typ |
68 Typ |
|||
| Spring | H08 |
77 Typ |
76 Typ |
2 Typ |
76 Typ |
70 Typ |
|||
| Tube | Light Drawn, Light Cold Rolled | H55 |
48 Typ |
36 Typ |
18 Typ |
67 Typ |
|||
| Nominal Grain Size 0.025 mm | OS025 |
41 Typ |
14 Typ |
46 Typ |
58 Typ |
||||
| Melting Point - Liquidus°F | 2050 |
|---|---|
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 14 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 37 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.7 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Good |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Good |
| Machinability Rating | 20 |
Common Fabrication Processes
- Forming and Bending
- Welding
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 1050 | 1500 | ||
| Hot Working Temperature | 1500 | 1750 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Condenser Plates | Corrosion Resistance | Corrosion Resistance to Fresh Water |
| Condenser Plates | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Condenser Plates | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Condenser Plates | Corrosion Resistance | Erosion and Impingement Corrosion Resistance | |
| Condenser Plates | Mechanical Properties | Moderate Strength | |
| Condenser Plates | Mechanical Properties | Retains Strength at High Temperatures | |
| Condensers | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Condensers | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Condensers | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Condensers | Corrosion Resistance | Erosion and Impingement Corrosion Resistance | |
| Condensers | Mechanical Properties | Moderate Strength | |
| Condensers | Mechanical Properties | Retains Strength at High Temperatures | |
| Evaporator Tubes | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Evaporator Tubes | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Evaporator Tubes | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Evaporator Tubes | Corrosion Resistance | Erosion and Impingement Corrosion Resistance | |
| Evaporator Tubes | Mechanical Properties | Moderate Strength | |
| Evaporator Tubes | Mechanical Properties | Retains Strength at High Temperatures | |
| Ferrules | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Ferrules | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Ferrules | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Ferrules | Corrosion Resistance | Erosion and Impingement Corrosion Resistance | |
| Ferrules | Mechanical Properties | Moderate Strength | |
| Ferrules | Mechanical Properties | Retains Strength at High Temperatures | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Heat Exchanger Tubes | Corrosion Resistance | Erosion and Impingement Corrosion Resistance | |
| Heat Exchanger Tubes | Mechanical Properties | Moderate Strength | |
| Heat Exchanger Tubes | Mechanical Properties | Retains Strength at High Temperatures | |
| Tubing for Lithium Bromide Absorption Systems | Corrosion Resistance | Corrosion Resistance | |
| Tubing for Lithium Bromide Absorption Systems | Corrosion Resistance | Erosion and Impingement Corrosion Resistance | |
| Tubing for Lithium Bromide Absorption Systems | Mechanical Properties | Moderate Strength | |
| Tubing for Lithium Bromide Absorption Systems | Mechanical Properties | Retains Strength at High Temperatures | |
| Marine | Condenser Intake Systems | Corrosion Resistance | Corrosion Resistance to Fresh Water |
| Condenser Intake Systems | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Condenser Intake Systems | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Condenser Intake Systems | Corrosion Resistance | Erosion and Impingement Corrosion Resistance | |
| Condenser Intake Systems | Mechanical Properties | Moderate Strength | |
| Condenser Intake Systems | Mechanical Properties | Retains Strength at High Temperatures | |
| Salt Water Piping | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Salt Water Piping | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Salt Water Piping | Corrosion Resistance | Erosion and Impingement Corrosion Resistance | |
| Salt Water Piping | Mechanical Properties | Moderate Strength | |
| Salt Water Piping | Mechanical Properties | Retains Strength at High Temperatures |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Condenser & Heat Exchanger Tube with Integral Fins | ASTM | B956/B956M | WELDED COPPER AND COPPER-ALLOY CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS | ||
| Pipe | ASTM | B466/B466M | SEAMLESS COPPER-NICKEL PIPE AND TUBE | ||
| Tube | ASME | SB359 | COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS | ||
| Condenser Tube | ASME | SB111 | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK | ||
| Condenser Tube | ASTM | B111/B111M | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK | ||
| ASME | SB466 | SEAMLESS COPPER-NICKEL PIPE AND TUBE | |||
| ASTM | B359/B359M | COPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS | |||
| ASME | SB543 | WELDED COPPER AND COPPER ALLOY TUBE | |||
| ASTM | B466/B466M | SEAMLESS COPPER-NICKEL PIPE AND TUBE | |||
| ASTM | B395/B395M | U-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES | |||
| ASTM | B543/B543M | WELDED COPPER AND COPPER ALLOY HEAT EXCHANGER TUBE |
Corrosion Properties