Find suppliers for this alloyC71000
Chemical Composition
Element
Cu(1,2)PbZnFeNi(3)Mn
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. (3) Ni value includes Co.
Min (%)19.0
Max (%)Rem0.051.01.023.01.0
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Fatigue Strength**
(ksi)
Section Size
(in)
Flat Products1/2 HardH0268   Typ
63   Typ
62   Typ
8   Typ
75   Typ
100   Typ
0.04
1/4 HardH0160   Typ
49   Typ
48   Typ
20   Typ
58   Typ
92   Typ
0.04
Extra HardH0678   Typ
76   Typ
75   Typ
4   Typ
82   Typ
0.04
Extra SpringH1085   Typ
79   Typ
78   Typ
3   Typ
86   Typ
0.04
HardH0475   Typ
72   Typ
71   Typ
5   Typ
80   Typ
0.04
Nominal Grain Size 0.025 mmOS02553   Typ
16   Typ
16   Typ
35   Typ
30   Typ
75   Typ
0.04
Nominal Grain Size 0.035 mmOS03552   Typ
14   Typ
14   Typ
35   Typ
27   Typ
73   Typ
0.04
Nominal Grain Size 0.050 mmOS05051   Typ
13   Typ
13   Typ
35   Typ
25   Typ
72   Typ
0.04
OS05051   Typ
13   Typ
35   Typ
0.04
SpringH0882   Typ
79   Typ
3   Typ
0.04
H0882   Typ
79   Typ
78   Typ
3   Typ
84   Typ
0.04
Flat Products & TubingNominal Grain Size 0.025 mmOS02553   Typ
16   Typ
35   Typ
0.04
OS02549   Typ
18   Typ
40   Typ
Flat Products & WireExtra SpringH1095   Typ
85   Typ
5   Typ
H1085   Typ
79   Typ
3   Typ
0.04
TubeLight Drawn, Light Cold RolledH5568   Typ
62   Typ
14   Typ
76   Typ
20   Typ
Nominal Grain Size 0.025 mmOS02549   Typ
18   Typ
40   Typ
72   Typ
WireExtra SpringH1095   Typ
85   Typ
5   Typ
0.08
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F2190
Melting Point - Solidus°F2100
Densitylb/cu in. at 68°F0.323
Specific Gravity8.94
Electrical Conductivity% IACS at 68°F6.5
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F21
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.1
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi20000
Modulus of Rigidityksi7500
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingExcellent
Coated Metal Arc WeldingGood
Spot WeldExcellent
Seam WeldExcellent
Butt WeldExcellent
Capacity for Being Cold WorkedGood
Capacity for Being Hot FormedGood
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Forming and Bending
  • Welding
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing12001500
Hot Treatment16001900
Typical uses
Product Category Product Reason Category Reason
ElectricalCommunication RelaysCorrosion ResistanceCorrosion Resistance
Communication RelaysForming CharacteristicsFormability
Communication RelaysMechanical PropertiesModerate Strength
Resistance WireConductivity (Electrical)Electrical Resistivity
Resistance WireMechanical PropertiesFlexibility
ResistorsCorrosion ResistanceCorrosion Resistance
ResistorsMechanical PropertiesModerate Strength
ResistorsSolderabilitySolderability
ResistorsWelding CharacteristicsWeldability
SpringsCorrosion ResistanceCorrosion Resistance
SpringsMechanical PropertiesHigh Modulus of Elasticity
SpringsMechanical PropertiesModerate Strength
IndustrialCondenser PlatesCorrosion ResistanceCorrosion Resistance
Condenser PlatesCorrosion ResistanceCorrosion Resistance to Salt Water
Condenser PlatesMechanical PropertiesModerate Strength
Condenser PlatesSolderabilitySolderability
Condenser PlatesWelding CharacteristicsWeldability
CondensersCorrosion ResistanceCorrosion Resistance
CondensersCorrosion ResistanceCorrosion Resistance to Salt Water
CondensersMechanical PropertiesModerate Strength
CondensersSolderabilitySolderability
CondensersWelding CharacteristicsWeldability
Evaporator TubingCorrosion ResistanceCorrosion Resistance
Evaporator TubingMechanical PropertiesModerate Strength
Evaporator TubingWelding CharacteristicsWeldability
EvaporatorsConductivity (Thermal)Thermal Conductivity
EvaporatorsCorrosion ResistanceCorrosion Resistance
EvaporatorsWelding CharacteristicsWeldability
FerrulesCorrosion ResistanceCorrosion Resistance
FerrulesCorrosion ResistanceCorrosion Resistance to Salt Water
FerrulesForming CharacteristicsFormability
FerrulesMechanical PropertiesModerate Strength
Heat Exchanger TubesCorrosion ResistanceCorrosion Resistance
Heat Exchanger TubesCorrosion ResistanceCorrosion Resistance to Salt Water
Heat Exchanger TubesForming CharacteristicsFormability
Heat Exchanger TubesMechanical PropertiesModerate Strength
Heat Exchanger TubesWelding CharacteristicsWeldability
Applicable Specifications
Form Specific Sub-Form Application System Standard Description
BarASTMB122/B122MCOPPER-NICKEL-ZINC ALLOY (NICKEL-SILVER) AND COPPER-NICKEL PLATE, SHEET, STRIP, AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
BoltsASTMF468NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE
Heat Exchanger TubeASMESB543WELDED COPPER AND COPPER ALLOY TUBE
NutsASTMF467NONFERROUS NUTS FOR GENERAL USE
PipeSeamlessASMESB466SEAMLESS COPPER-NICKEL PIPE AND TUBE
SeamlessASTMB466/B466MSEAMLESS COPPER-NICKEL PIPE AND TUBE
PlateASTMB122/B122MCOPPER-NICKEL-ZINC ALLOY (NICKEL-SILVER) AND COPPER-NICKEL PLATE, SHEET, STRIP, AND ROLLED BAR
ScrewsASTMF468NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE
SheetASTMB122/B122MCOPPER-NICKEL-ZINC ALLOY (NICKEL-SILVER) AND COPPER-NICKEL PLATE, SHEET, STRIP, AND ROLLED BAR
ASTMB694COPPER, COPPER ALLOY AND COPPER-CLAD STAINLESS STEEL SHEET AND STRIP FOR ELECTRICAL CABLE SHIELDING
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
StripASTMB122/B122MCOPPER-NICKEL-ZINC ALLOY (NICKEL-SILVER) AND COPPER-NICKEL PLATE, SHEET, STRIP, AND ROLLED BAR
ASTMB694COPPER, COPPER ALLOY AND COPPER-CLAD STAINLESS STEEL SHEET AND STRIP FOR ELECTRICAL CABLE SHIELDING
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
StudsASTMF468NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE
TubeCondenser TubeASMESB111COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK
FinnedASMESB359COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS
U-BendASMESB395U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE
SeamlessASMESB466SEAMLESS COPPER-NICKEL PIPE AND TUBE
Condenser TubeASTMB111/B111MCOPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK
FinnedASTMB359/B359MCOPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
U-BendASTMB395/B395MU-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES
SeamlessASTMB466/B466MSEAMLESS COPPER-NICKEL PIPE AND TUBE
ASTMB543/B543MWELDED COPPER AND COPPER ALLOY HEAT EXCHANGER TUBE
Condenser TubeSAEJ461WROUGHT AND CAST COPPER ALLOYS
Condenser TubeSAEJ463WROUGHT COPPER AND COPPER ALLOYS
Welded Heat Exchanger & Condenser TubeASTMB956/B956MWELDED COPPER AND COPPER-ALLOY CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS
WireASTMB206/B206MCOPPER-NICKEL-ZINC ALLOY (NICKEL-SILVER WIRE) AND COPPER-NICKEL ALLOY WIRE
Corrosion Properties

No information available.