| Elements | |||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Fe | P | Ni | B | Bi | C | Co | Cr | Mn | S | Si | Ti | Zr | |
|
(1) Cu + Sum of Named Elements 99.93% min. |
|||||||||||||||
| Min (%) | 0.5 | 29.0 | 1.6 | 0.5 | 0.20 | 0.03 | 0.05 | ||||||||
| Max (%) | Rem | 0.005 | 1.0 | 0.005 | 32.0 | 0.001 | 0.001 | 0.020 | 0.050 | 2.0 | 1.0 | 0.005 | 0.40 | 0.15 | 0.15 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load | Shear Strength (ksi) |
Impact Strength (ft-lbs) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| Rod, Bar & Forging | Spinodal Hardened-Low Strength (ATLS) | TX00 |
80 Min 87 Typ 119 Max |
51 Min 61 Typ 105 Max |
20 Min 27 Max |
170 Min 250 Max |
39 Typ |
81.13 Typ |
| Melting Point - Liquidus°F | 2204 |
|---|---|
| Melting Point - Solidus°F | 2120 |
| Densitylb/cu in. at 68°F | 0.318 |
| Specific Gravity | 8.8 |
| Electrical Conductivity% IACS at 68°F | 4 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 13.3 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
| Modulus of Elasticity in Tensionksi | 20200 |
| Modulus of Rigidityksi | 782 |
| Magnetic Permeability | 1.01 |
| Poisson's Ratio | 0.3 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties