| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | Ni(2) | Mg | Mn | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Includes Co. |
||||||||
| Min (%) | 4.5 | 7.0 | .05 | |||||
| Max (%) | Rem | .02 | 5.5 | .50 | .50 | 8.0 | .15 | .30 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Vickers Hardness, 500 gm | Vickers Hardness, 3000 gm |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Rod | 1/2 Hard and Spinodal Hardened (1/2 TS) | TS02 |
66.7 Min 69.6 Typ 72.5 Max |
53.7 Min 61.6 Typ |
160 Typ |
|
| 1/4 Hard and Spinodal Hardened (1/4 TS) | TS01 |
105.9 Min 115.3 Typ 124.7 Max |
91.4 Min 102.3 Typ |
270 Typ |
||
| Precipitation Heat Treated or Spinodal Heat Treated and 1/4 Hard | TL01 |
113.1 Min 117.5 Typ 121.8 Max |
79.8 Min 94.3 Typ |
280 Typ |
||
| Precipitation Heat Treated or Spinodal Heat Treated and Spring | TL08 |
137.8 Min 148.7 Typ 159.5 Max |
132 Min 144.3 Typ |
330 Typ |
||
| Wire | 1/2 Hard and Spinodal Hardened (1/2 TS) | TS02 |
72.5 Min 79.8 Typ 87.0 Max |
69.6 Min 74.0 Typ |
200 Typ |
|
| 1/4 Hard and Spinodal Hardened (1/4 TS) | TS01 |
66.7 Min 67.6 Typ 72.5 Max |
53.7 Min 61.6 Typ |
|||
| 3/4 Hard and Spinodal Hardened (3/4 TS) | TS03 |
87.0 Min 92.8 Typ 98.6 Max |
78.3 Min 83.4 Typ |
220 Typ |
||
| Quench Hardened | TQ00 |
59.5 Min 63.8 Typ 66.7 Max |
53.7 Typ |
140 Max | ||
| Spinodal Hardened-Low Strength (ATLS) | TX00 |
107.3 Typ |
95.7 Typ |
240 Typ |
||
| Spring and Spinodal Hardened | TS08 |
98.6 Min 103.0 Typ 107.3 Max |
88.5 Min 92.1 Typ |
240 Typ |
||
| Melting Point - Solidus°F | 1760 |
|---|---|
| Densitylb/cu in. at 68°F | 0.318 |
| Specific Gravity | 8.8 |
| Electrical Conductivity% IACS at 68°F | 13 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 31.7 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Spot Weld | Fair |
| Seam Weld | Fair |
| Butt Weld | Fair |
| Capacity for Being Cold Worked | Excellent |
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Conductors | ||
| Connector Components | |||
| Industrial | Screw Machine Parts, Products |
Applicable Specifications
Corrosion Properties