Find suppliers for this alloy
C79360
Elements | |||||||
---|---|---|---|---|---|---|---|
Cu(1) | Pb | Sn | Zn | Fe | Ni | Mn | |
(1) Cu + Sum of Named Elements 99.5% min. |
|||||||
Min (%) | 55.0 | 24.0 | |||||
Max (%) | 57.0 | 0.03 | 0.20 | Rem | 0.30 | 26.0 | 0.50 |
Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
---|---|---|---|---|---|
* Measured at room temperature, 68°F (20°C). | |||||
Flat Products | Super Spring | H12 |
65.3 Min 79.8 Max |
58.0 Max | 5.0 Max |
Ultra Spring | H13 |
74.5 Min 87.0 Max |
72.5 Max | 1.0 Max | |
Super Spring | H14 |
84.1 Min |
79.8 Max | 1.0 Max | |
Rod & Bar | Special Spring | H12 |
72.5 Min 79.8 Max |
2.0 Max | |
Ultra Spring | H13 |
79.8 Min 87.0 Max |
1.0 Max | ||
Super Spring | H14 |
79.8 Min 101.5 Max |
|||
Wire | Super Spring | H12 |
94.3 Min 108.8 Max |
2.0 Max | |
Ultra Spring | H13 |
101.5 Min 118.9 Max |
1.0 Max | ||
Super Spring | H14 |
116.0 Min 118.0 Max |
Melting Point - Liquidus°F | 2102 |
---|---|
Densitylb/cu in. at 68°F | .318 |
Specific Gravity | 8.8 |
Electrical Conductivity% IACS at 68°F | 4.6 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 12.7 |
Modulus of Elasticity in Tensionksi | 24000 |
Technique | Suitability |
---|---|
Soldering | Excellent |
Brazing | Excellent |
Oxyacetylene Welding | Excellent |
Gas Shielded Arc Welding | Excellent |
Spot Weld | Excellent |
Seam Weld | Excellent |
Butt Weld | Excellent |
Capacity for Being Cold Worked | Excellent |
Capacity for Being Hot Formed | Excellent |
Common Fabrication Processes
Typical Uses
Applicable Specifications
Corrosion Properties