SSL certificate problem: certificate has expired
Find suppliers for this alloy C81700
Chemical Composition
Elements
Cu(1) Ni Ag Be Co
(1) Cu + Sum of Named Elements 99.5% min.
Min (%) 94.2 0.25 0.8 0.30 0.25
Max (%) 1.5 1.2 0.55 1.5
Mechanical Properties *
Form Temper Temper Code Tensile Strength
(ksi)
YS-0.2% Offset
(ksi)
Elongation
(%)
Brinell Hardness, 3000 kg load Shear Strength
(ksi)
Izod
(ft-lbs)
Charpy V-Notch Impact Strength
(ft-lbs)
Compressive Strength .1 in. set/in.
(ksi)
Fatigue Strength**
(ksi)
Proportional Limit
(ksi)
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
As Sand Cast As Sand Cast M01 92 Typ
68 Typ
8 Typ
217 Typ
70 Typ
8 Typ 12 Typ
80 Typ 17 Typ 50 Typ
Physical Properties
Melting Point - Liquidus°F 1955
Melting Point - Solidus°F 1885
Densitylb/cu in. at 68°F 0.316
Specific Gravity 8.75
Electrical Conductivity% IACS at 68°F 48
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F 109
Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) 9.5
Specific Heat CapacityBtu/ lb /°F at 68°F 0.1
Modulus of Elasticity in Tensionksi 17000
Casting Characteristics
Casting Attribute Level
Casting Yield Medium
Drossing Low
Effect of Section Size Low
Fluidity High
Gassing Medium
Patternmakers Shrinkage inches per inch 3/16
Shrinkage in Solidification High
Fabrication Properties
Technique Suitability
Soldering Good
Brazing Good
Oxyacetylene Welding Not Recommended
Gas Shielded Arc Welding Fair
Coated Metal Arc Welding Not Recommended
Machinability Rating 30
Common Fabrication Processes

No fabrication process properties for this alloy

Thermal Properties
Treatment Minimum* Maximum* Value* Time** Medium
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief 500
Solution Treatment 1650 1700 1 Water
Precipitation Treatment 850 3 Air
Typical Uses

No information for this alloy

Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties