Chemical Composition
Elements
Cu(1) Ni Be Co Si
(1) Cu + Sum of Named Elements 99.5% min.
Min (%) 1.0 0.35
Max (%) Rem 3.0 0.8 0.30 0.15
Mechanical Properties *
Form Temper Temper Code Tensile Strength
(ksi)
YS-0.2% Offset
(ksi)
Elongation
(%)
Rockwell B scale Proportional Limit
(ksi)
* Measured at room temperature, 68°F (20°C).
As Sand Cast As Cast and Precipitation Heat Treated O11 65 Typ
40 Typ
15 Typ
75 Typ
As Sand Cast M01 55 Min for Standard
55 Typ
25 Min for Standard
30 Typ
15 Min for Standard
20 Typ
55 Typ
20 Typ
Precipitation Hardened TF00 90 Min for Standard
100 Typ
70 Min for Standard
75 Typ
5 Min for Standard
7 Typ
96 Typ
Solution Heat Treated TB00 45 Typ
12 Typ
30 Typ
30 Typ
Physical Properties
(1)TF00 Condition
Melting Point - Liquidus°F 1970
Melting Point - Solidus°F 1900
Densitylb/cu in. at 68°F 0.316 (1)
Specific Gravity 8.75
Electrical Conductivity% IACS at 68°F 45
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F 106
Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) 9.6
Specific Heat CapacityBtu/ lb /°F at 68°F 0.1
Modulus of Elasticity in Tensionksi 20000
Change in Density During Aging% 0.6
Magnetic Permeability 1.001
Poisson's Ratio 0.33
Casting Characteristics
Casting Attribute Level
Casting Yield Medium
Drossing Low
Effect of Section Size Low
Fluidity Medium
Gassing Medium
Patternmakers Shrinkage inches per inch 3/16
Shrinkage in Solidification Medium
Shrinkage During Aging 0.2
Fabrication Properties
Technique Suitability
Soldering Good
Brazing Good
Oxyacetylene Welding Not Recommended
Gas Shielded Arc Welding Fair
Coated Metal Arc Welding Fair
Machinability Rating 30
Common Fabrication Processes

No fabrication process properties for this alloy

Thermal Properties
Treatment Minimum* Maximum* Value* Time** Medium
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief 500
Solution Treatment 1650 1700 0.5 Water
Precipitation Treatment 850 3 Air
Typical uses
Product Category Product Reason Category Reason
Automotive Brake Drums Conductivity (Thermal) Thermal Conductivity
Brake Drums Corrosion Resistance Corrosion Resistance
Brake Drums Corrosion Resistance Oxidation Resistance
Brake Drums Mechanical Properties Moderate Strength
Electrical Aerospace Components Requiring Non-Sparking Action Conductivity (Electrical) Electrical Conductivity
Aerospace Components Requiring Non-Sparking Action Conductivity (Thermal) Thermal Conductivity
Aerospace Components Requiring Non-Sparking Action Corrosion Resistance Corrosion Resistance
Aerospace Components Requiring Non-Sparking Action Corrosion Resistance Oxidation Resistance
Aerospace Components Requiring Non-Sparking Action Mechanical Properties High Strength
Contacts Conductivity (Electrical) Electrical Conductivity
Contacts Conductivity (Thermal) Thermal Conductivity
Contacts Friction & Wear Properties Wear Resistance
Contacts Mechanical Properties High Strength
Electrical Switches Conductivity (Electrical) Electrical Conductivity
Electrical Switches Conductivity (Thermal) Thermal Conductivity
Electrical Switches Corrosion Resistance Corrosion Resistance
Electrical Switches Friction & Wear Properties Wear Resistance
Electrical Switches Mechanical Properties High Strength
Military Components Requiring Non-Sparking Action Conductivity (Electrical) Electrical Conductivity
Military Components Requiring Non-Sparking Action Conductivity (Thermal) Thermal Conductivity
Military Components Requiring Non-Sparking Action Friction & Wear Properties Wear Resistance
Military Components Requiring Non-Sparking Action Mechanical Properties High Strength
Industrial Beam Welder Shapes Conductivity (Electrical) Electrical Conductivity
Beam Welder Shapes Conductivity (Thermal) Thermal Conductivity
Beam Welder Shapes Corrosion Resistance Corrosion Resistance
Beam Welder Shapes Corrosion Resistance Oxidation Resistance
Beam Welder Shapes Mechanical Properties Moderate Strength
Bushings Corrosion Resistance Corrosion Resistance
Bushings Corrosion Resistance Oxidation Resistance
Bushings Friction & Wear Properties Anti-Seizing Properties
Bushings Friction & Wear Properties Low Coefficient of Friction
Bushings Mechanical Properties Moderate Strength
Clutch Rings Corrosion Resistance Corrosion Resistance
Clutch Rings Corrosion Resistance Oxidation Resistance
Clutch Rings Mechanical Properties Moderate Strength
Seam Welder Electrodes Conductivity (Electrical) Electrical Conductivity
Seam Welder Electrodes Conductivity (Thermal) Thermal Conductivity
Seam Welder Electrodes Corrosion Resistance Corrosion Resistance
Seam Welder Electrodes Corrosion Resistance Oxidation Resistance
Seam Welder Electrodes Mechanical Properties Moderate Strength
Spot Welding Tips Conductivity (Electrical) Electrical Conductivity
Spot Welding Tips Conductivity (Thermal) Thermal Conductivity
Spot Welding Tips Corrosion Resistance Corrosion Resistance
Spot Welding Tips Corrosion Resistance Oxidation Resistance
Spot Welding Tips Mechanical Properties Moderate Strength
Water Cooled Holders Conductivity (Thermal) Thermal Conductivity
Water Cooled Holders Corrosion Resistance Corrosion Resistance
Water Cooled Holders Corrosion Resistance Oxidation Resistance
Water Cooled Holders Mechanical Properties Moderate Strength
Applicable Specifications
Form Specific Sub-Form Application System Standard Description
As Sand Cast Castings ASTM B770 COPPER-BERYLLIUM SAND CASTINGS
Ingot ASTM B30 COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties

No Corrosion Properties Available.