Find suppliers for this alloy
C82600
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | Ni | Al | Be | Co | Cr | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||||||||||
| Min (%) | 2.25 | 0.35 | 0.20 | ||||||||
| Max (%) | Rem | 0.02 | 0.10 | 0.10 | 0.25 | 0.20 | 0.15 | 2.55 | 0.65 | 0.09 | 0.35 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell C scale | Torsion Modulus (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| As Sand Cast | As Cast and Precipitation Heat Treated | O11 |
120 Typ |
105 Typ |
2 Typ |
31 Typ |
||
| As Sand Cast | M01 |
80 Min for Standard |
45 Min for Standard 50 Typ |
10 Min for Standard |
86 Typ |
|||
| Precipitation Hardened | TF00 |
165 Min for Standard |
155 Min for Standard |
1 Min for Standard |
45 Typ |
7.3 Typ | ||
| Solution Heat Treated | TB00 |
70 Typ |
30 Typ |
12 Typ |
75 Typ |
|||
| (1)TF00 Condition(2)+ .002 | |
| Melting Point - Liquidus°F | 1750 |
|---|---|
| Melting Point - Solidus°F | 1575 |
| Densitylb/cu in. at 68°F | 0.292 (1) |
| Specific Gravity | 8.09 |
| Electrical Conductivity% IACS at 68°F | 19 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 73 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.4 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.1 |
| Modulus of Elasticity in Tensionksi | 19000 |
| Change in Density During Aging% | 0.6 |
| Incipient Melting°F | 1535 |
| Magnetic Permeability | 1.002 (2) |
| Poisson's Ratio | 0.3 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | Medium |
| Fluidity | High |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Medium |
| Shrinkage During Aging | 0.2 |
| Technique | Suitability |
|---|---|
| Soldering | Fair |
| Brazing | Fair |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Fair |
| Machinability Rating | 30 |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | Value* | Time** | Medium |
|---|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | |||||
| Precipitation Treatment | 650 | 3 | Air | ||
| Solution Treatment | 1400 | 1475 | 0.5 | Water | |
| Stress Relief | 500 | ||||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Architecture | Sculpture | Appearance | Appearance |
| Sculpture | Casting Characteristics | Castability | |
| Sculpture | Corrosion Resistance | Corrosion Resistance | |
| Consumer | Golf Clubs | Corrosion Resistance | Corrosion Resistance |
| Golf Clubs | Mechanical Properties | High Modulus of Elasticity | |
| Golf Clubs | Mechanical Properties | Very High Strength | |
| Jewelry | Appearance | Appearance | |
| Jewelry | Casting Characteristics | Castability | |
| Jewelry | Corrosion Resistance | Corrosion Resistance | |
| Jewelry | Mechanical Properties | Ductility | |
| Safety Tools | Corrosion Resistance | Corrosion Resistance | |
| Safety Tools | Mechanical Properties | Very High Strength | |
| Safety Tools | Non-Magnetic | Non-Magnetic | |
| Safety Tools | Non-Sparking | Non-Sparking | |
| Industrial | Aluminum Die Cast Plunger Tips | Conductivity (Thermal) | Thermal Conductivity |
| Aluminum Die Cast Plunger Tips | Corrosion Resistance | Corrosion Resistance | |
| Aluminum Die Cast Plunger Tips | Mechanical Properties | Very High Strength | |
| Condenser Tube Plates | Conductivity (Thermal) | Thermal Conductivity | |
| Condenser Tube Plates | Corrosion Resistance | Corrosion Resistance | |
| Condenser Tube Plates | Mechanical Properties | Very High Strength | |
| Condenser Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Condenser Tubes | Corrosion Resistance | Corrosion Resistance | |
| Condenser Tubes | Mechanical Properties | Very High Strength | |
| Corrosion Resistant Valves | Corrosion Resistance | Corrosion Resistance | |
| Corrosion Resistant Valves | Corrosion Resistance | Corrosion Resistance to Most Chemical Environments | |
| Corrosion Resistant Valves | Corrosion Resistance | Resists Stress Corrosion Cracking in Many Chemical Environments | |
| Corrosion Resistant Valves | Corrosion Resistance | Resists Stress Corrosion Cracking in Marine Environments | |
| Corrosion Resistant Valves | Friction & Wear Properties | Wear Resistance | |
| Corrosion Resistant Valves | Mechanical Properties | Very High Strength | |
| Distiller Ferrules | Corrosion Resistance | Corrosion Resistance | |
| Distiller Ferrules | Mechanical Properties | Ductility | |
| Distiller Ferrules | Mechanical Properties | Very High Strength | |
| Distiller Tubes | Corrosion Resistance | Corrosion Resistance | |
| Distiller Tubes | Mechanical Properties | Ductility | |
| Distiller Tubes | Mechanical Properties | Very High Strength | |
| Evaporator Tubes | Conductivity (Thermal) | Thermal Conductivity | |
| Evaporator Tubes | Corrosion Resistance | Corrosion Resistance | |
| Evaporator Tubes | Mechanical Properties | Very High Strength | |
| Glass Molds | Conductivity (Thermal) | Thermal Conductivity | |
| Glass Molds | Corrosion Resistance | Corrosion Resistance | |
| Glass Molds | Friction & Wear Properties | Wear Resistance | |
| Glass Molds | Mechanical Properties | Very High Strength | |
| Heat Exchanger Tube | Conductivity (Thermal) | Thermal Conductivity | |
| Heat Exchanger Tube | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tube | Mechanical Properties | Very High Strength | |
| Molds for Plastic Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Molds for Plastic Parts | Corrosion Resistance | Corrosion Resistance | |
| Molds for Plastic Parts | Friction & Wear Properties | Wear Resistance | |
| Molds for Plastic Parts | Mechanical Properties | Very High Strength | |
| Permanent Molds for Aluminum Castings | Conductivity (Thermal) | Thermal Conductivity | |
| Permanent Molds for Aluminum Castings | Corrosion Resistance | Corrosion Resistance | |
| Permanent Molds for Aluminum Castings | Friction & Wear Properties | Wear Resistance | |
| Permanent Molds for Aluminum Castings | Mechanical Properties | Very High Strength | |
| Permanent Molds for Brass Casting | Conductivity (Thermal) | Thermal Conductivity | |
| Permanent Molds for Brass Casting | Corrosion Resistance | Corrosion Resistance | |
| Permanent Molds for Brass Casting | Friction & Wear Properties | Wear Resistance | |
| Permanent Molds for Brass Casting | Mechanical Properties | Very High Strength | |
| Pressure Housings in Salt Water Environments | Corrosion Resistance | Corrosion Resistance | |
| Pressure Housings in Salt Water Environments | Corrosion Resistance | Resists Stress Corrosion Cracking in Marine Environments | |
| Pressure Housings in Salt Water Environments | Mechanical Properties | High Strength | |
| Marine | Undersea Cable Housing | Conductivity (Electrical) | Electrical Conductivity |
| Undersea Cable Housing | Corrosion Resistance | Corrosion Resistance | |
| Undersea Cable Housing | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Undersea Cable Housing | Mechanical Properties | Very High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Sand Cast | Castings | ASTM | B770 | COPPER-BERYLLIUM SAND CASTINGS | |
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
| Valves |
Corrosion Properties