Chemical Composition
Element
Cu(1)PbSnZnFeNiAlBeCoCrSi
(1) Cu + Sum of Named Elements 99.5% min.
Min (%)2.250.350.20
Max (%)Rem0.020.100.100.250.200.152.550.650.090.35
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
Elongation
(%)
Rockwell B scale
Rockwell C scale
Torsion Modulus
(ksi)
As Sand CastAs Cast and Precipitation Heat TreatedO11120   Typ
105   Typ
2   Typ
31   Typ
As Sand CastM0180   Min for Standard
45   Min for Standard
50   Typ
10   Min for Standard
86   Typ
Precipitation HardenedTF00165   Min for Standard
155   Min for Standard
1   Min for Standard
45   Typ
7.3   Typ
Solution Heat TreatedTB0070   Typ
30   Typ
12   Typ
75   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) TF00 Condition
(2) + .002
Melting Point - Liquidus°F1750
Melting Point - Solidus°F1575
Densitylb/cu in. at 68°F0.292(1)
Specific Gravity8.09
Electrical Conductivity% IACS at 68°F19
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F73
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)9.4
Specific Heat CapacityBtu/ lb /°F at 68°F0.1
Modulus of Elasticity in Tensionksi19000
Change in Density During Aging%0.6
Incipient Melting°F1535
Magnetic Permeability1.002(2)
Poisson's Ratio0.3
Casting Characteristics
Casting Attribute Level
Casting YieldHigh
DrossingLow
Effect of Section SizeMedium
FluidityHigh
GassingMedium
Patternmakers Shrinkageinches per inch3/16
Shrinkage in SolidificationMedium
Shrinkage During Aging0.2
Fabrication Properties
Technique Suitability
SolderingFair
BrazingFair
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingFair
Machinability Rating30
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Minimum* Maximum* Value* Time** Medium
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief500
Solution Treatment140014750.5Water
Precipitation Treatment6503Air
Typical uses
Product Category Product Reason Category Reason
ArchitectureSculptureAppearanceAppearance
SculptureCasting CharacteristicsCastability
SculptureCorrosion ResistanceCorrosion Resistance
ConsumerGolf ClubsCorrosion ResistanceCorrosion Resistance
Golf ClubsMechanical PropertiesHigh Modulus of Elasticity
Golf ClubsMechanical PropertiesVery High Strength
JewelryAppearanceAppearance
JewelryCasting CharacteristicsCastability
JewelryCorrosion ResistanceCorrosion Resistance
JewelryMechanical PropertiesDuctility
Safety ToolsCorrosion ResistanceCorrosion Resistance
Safety ToolsMechanical PropertiesVery High Strength
Safety ToolsNon-MagneticNon-Magnetic
Safety ToolsNon-SparkingNon-Sparking
IndustrialAluminum Die Cast Plunger TipsConductivity (Thermal)Thermal Conductivity
Aluminum Die Cast Plunger TipsCorrosion ResistanceCorrosion Resistance
Aluminum Die Cast Plunger TipsMechanical PropertiesVery High Strength
Condenser Tube PlatesConductivity (Thermal)Thermal Conductivity
Condenser Tube PlatesCorrosion ResistanceCorrosion Resistance
Condenser Tube PlatesMechanical PropertiesVery High Strength
Condenser TubesConductivity (Thermal)Thermal Conductivity
Condenser TubesCorrosion ResistanceCorrosion Resistance
Condenser TubesMechanical PropertiesVery High Strength
Corrosion Resistant ValvesCorrosion ResistanceCorrosion Resistance
Corrosion Resistant ValvesCorrosion ResistanceCorrosion Resistance to Most Chemical Environments
Corrosion Resistant ValvesCorrosion ResistanceResists Stress Corrosion Cracking in Many Chemical Environments
Corrosion Resistant ValvesCorrosion ResistanceResists Stress Corrosion Cracking in Marine Environments
Corrosion Resistant ValvesFriction & Wear PropertiesWear Resistance
Corrosion Resistant ValvesMechanical PropertiesVery High Strength
Distiller FerrulesCorrosion ResistanceCorrosion Resistance
Distiller FerrulesMechanical PropertiesDuctility
Distiller FerrulesMechanical PropertiesVery High Strength
Distiller TubesCorrosion ResistanceCorrosion Resistance
Distiller TubesMechanical PropertiesDuctility
Distiller TubesMechanical PropertiesVery High Strength
Evaporator TubesConductivity (Thermal)Thermal Conductivity
Evaporator TubesCorrosion ResistanceCorrosion Resistance
Evaporator TubesMechanical PropertiesVery High Strength
Glass MoldsConductivity (Thermal)Thermal Conductivity
Glass MoldsCorrosion ResistanceCorrosion Resistance
Glass MoldsFriction & Wear PropertiesWear Resistance
Glass MoldsMechanical PropertiesVery High Strength
Heat Exchanger TubeConductivity (Thermal)Thermal Conductivity
Heat Exchanger TubeCorrosion ResistanceCorrosion Resistance
Heat Exchanger TubeMechanical PropertiesVery High Strength
Molds for Plastic PartsConductivity (Thermal)Thermal Conductivity
Molds for Plastic PartsCorrosion ResistanceCorrosion Resistance
Molds for Plastic PartsFriction & Wear PropertiesWear Resistance
Molds for Plastic PartsMechanical PropertiesVery High Strength
Permanent Molds for Aluminum CastingsConductivity (Thermal)Thermal Conductivity
Permanent Molds for Aluminum CastingsCorrosion ResistanceCorrosion Resistance
Permanent Molds for Aluminum CastingsFriction & Wear PropertiesWear Resistance
Permanent Molds for Aluminum CastingsMechanical PropertiesVery High Strength
Permanent Molds for Brass CastingConductivity (Thermal)Thermal Conductivity
Permanent Molds for Brass CastingCorrosion ResistanceCorrosion Resistance
Permanent Molds for Brass CastingFriction & Wear PropertiesWear Resistance
Permanent Molds for Brass CastingMechanical PropertiesVery High Strength
Pressure Housings in Salt Water EnvironmentsCorrosion ResistanceCorrosion Resistance
Pressure Housings in Salt Water EnvironmentsCorrosion ResistanceResists Stress Corrosion Cracking in Marine Environments
Pressure Housings in Salt Water EnvironmentsMechanical PropertiesHigh Strength
MarineUndersea Cable HousingConductivity (Electrical)Electrical Conductivity
Undersea Cable HousingCorrosion ResistanceCorrosion Resistance
Undersea Cable HousingCorrosion ResistanceCorrosion Resistance to Salt Water
Undersea Cable HousingMechanical PropertiesVery High Strength
Applicable Specifications
Form Sub-Form System Standard Description
As Sand CastCastingsASTMB770COPPER-BERYLLIUM SAND CASTINGS
IngotASTMB30COPPER BASE ALLOYS IN INGOT FORM
Valves
Corrosion Properties

No information available.