Find suppliers for this alloy
C83400
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) Cu + Sum of Named Elements 99.3% min. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 88.0 | 8.0 | |||||||||
| Max (%) | 92.0 | 0.50 | 0.20 | 12.0 | 0.25 | 0.03 | 1.0 | 0.005 | 0.08 | 0.25 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell F scale | Shear Strength (ksi) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| As Sand Cast | As Sand Cast | M01 |
35 Typ |
10 Typ |
30 Typ |
50 Typ |
26 Typ |
| Melting Point - Liquidus°F | 1910 |
|---|---|
| Melting Point - Solidus°F | 1870 |
| Densitylb/cu in. at 68°F | 0.318 |
| Specific Gravity | 8.8 |
| Electrical Conductivity% IACS at 68°F | 44 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 109 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 15000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | Low |
| Fluidity | Medium |
| Gassing | Low |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Medium |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 60 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Rotating Bands | Conductivity (Thermal) | Thermal Conductivity |
| Rotating Bands | Corrosion Resistance | Corrosion Resistance | |
| Rotating Bands | Friction & Wear Properties | Wear Resistance | |
| Rotating Bands | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bands | Projectile Rotating | MILITARY | MIL-B-46066 | BANDS, ROTATING, COPPER ALLOY CENTRIFUGAL CAST (FOR CRITICAL APPLICATIONS) |
Corrosion Properties