| Elements | ||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni | Al | B | Mn | S | Sb | Si | Zr | |
|
(1) Cu + Sum of Named Elements 99.3% min. |
||||||||||||||
| Min (%) | 82.0 | 2.0 | 5.0 | 0.50 | 0.01 | 0.10 | ||||||||
| Max (%) | 89.0 | 0.09 | 4.0 | 14.0 | 0.40 | 0.05 | 2.0 | 0.005 | 0.10 | 0.20 | 0.65 | 0.02 | 0.005 | 0.10 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Castings | As Sand Cast | M01 |
34.5 Min 38.5 Typ |
15 Min 18 Typ |
17 Min 30.5 Typ |
65 Typ |
| Melting Point - Liquidus°F | 1895 |
|---|---|
| Melting Point - Solidus°F | 1722 |
| Densitylb/cu in. at 68°F | 0.309 |
| Specific Gravity | 8.55 |
| Electrical Conductivity% IACS at 68°F | 16 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 41.8 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.094 |
| Modulus of Elasticity in Tensionksi | 14700 |
| Magnetic Permeability | 1 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Medium |
| Effect of Section Size | High |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Medium |