| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.3% min. (2) In determining Cu min., Cu may be calculated as Cu + Ni. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 78.0 | 2.0 | 4.0 | 10.0 | |||||||
| Max (%) | 82.0 | 3.0 | 6.0 | 16.0 | 0.40 | 0.05 | 0.8 | 0.005 | 0.08 | 0.25 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| As Continuous Cast | As Continuous Cast | M07 |
32 Min for Standard |
16 Min for Standard |
13 Min for Standard |
|
| As Sand Cast | As Sand Cast | M01 |
35 Typ |
14 Typ |
27 Typ |
60 Typ |
| Melting Point - Liquidus°F | 1820 |
|---|---|
| Melting Point - Solidus°F | 1540 |
| Densitylb/cu in. at 68°F | 0.311 |
| Specific Gravity | 8.61 |
| Electrical Conductivity% IACS at 68°F | 16.4 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 41.8 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 14000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | High |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Fair |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Builders Hardware | General Hardware | Appearance | Appearance |
| General Hardware | Corrosion Resistance | Corrosion Resistance | |
| General Hardware | Machining Properties | Machinability, Good | |
| General Hardware | Mechanical Properties | Moderate Strength | |
| Industrial | Bushings | Corrosion Resistance | Corrosion Resistance |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Machining Properties | Machinability, Good | |
| Bushings | Mechanical Properties | Moderate Strength | |
| Fittings for Gas Lines | Corrosion Resistance | Corrosion Resistance | |
| Fittings for Gas Lines | Machining Properties | Machinability, Good | |
| Fittings for Gas Lines | Mechanical Properties | Moderate Strength | |
| Fittings for Gas Lines | Pressure Tight | Pressure Tight | |
| Fittings for Oil Lines | Corrosion Resistance | Corrosion Resistance | |
| Fittings for Oil Lines | Machining Properties | Machinability, Good | |
| Fittings for Oil Lines | Mechanical Properties | Moderate Strength | |
| Fittings for Oil Lines | Pressure Tight | Pressure Tight | |
| Low Pressure Valves | Corrosion Resistance | Corrosion Resistance | |
| Low Pressure Valves | Friction & Wear Properties | Wear Resistance | |
| Low Pressure Valves | Machining Properties | Machinability, Good | |
| Low Pressure Valves | Mechanical Properties | Moderate Strength | |
| Small Gears | Corrosion Resistance | Corrosion Resistance | |
| Small Gears | Friction & Wear Properties | Wear Resistance | |
| Small Gears | Machining Properties | Machinability, Good | |
| Small Gears | Mechanical Properties | Moderate Strength | |
| Small Pump Castings | Corrosion Resistance | Corrosion Resistance | |
| Small Pump Castings | Machining Properties | Machinability, Good | |
| Small Pump Castings | Mechanical Properties | Moderate Strength | |
| Small Pump Castings | Pressure Tight | Pressure Tight | |
| Plumbing | Couplings | Corrosion Resistance | Corrosion Resistance |
| Couplings | Friction & Wear Properties | Wear Resistance | |
| Couplings | Machining Properties | Machinability, Good | |
| Couplings | Mechanical Properties | Moderate Strength | |
| Elbows | Corrosion Resistance | Corrosion Resistance | |
| Elbows | Friction & Wear Properties | Wear Resistance | |
| Elbows | Machining Properties | Machinability, Good | |
| Elbows | Mechanical Properties | Moderate Strength | |
| Pipe Fittings | Corrosion Resistance | Corrosion Resistance | |
| Pipe Fittings | Machining Properties | Machinability, Good | |
| Pipe Fittings | Mechanical Properties | Moderate Strength | |
| Pipe Fittings | Pressure Tight | Pressure Tight | |
| Plugs | Corrosion Resistance | Corrosion Resistance | |
| Plugs | Friction & Wear Properties | Wear Resistance | |
| Plugs | Machining Properties | Machinability, Good | |
| Plugs | Mechanical Properties | Moderate Strength | |
| Tees | Corrosion Resistance | Corrosion Resistance | |
| Tees | Friction & Wear Properties | Wear Resistance | |
| Tees | Machining Properties | Machinability, Good | |
| Tees | Mechanical Properties | Moderate Strength | |
| Unions | Corrosion Resistance | Corrosion Resistance | |
| Unions | Friction & Wear Properties | Wear Resistance | |
| Unions | Machining Properties | Machinability, Good | |
| Unions | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Continuous Cast | Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | |
| Fitting | FEDERAL | WW-P-460 | PIPE FITTINGS: BRASS OR BRONZE | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties