SSL certificate problem: certificate has expired
Find suppliers for this alloy C85200
Chemical Composition
Elements
Cu(1,2) Pb Sn Zn Fe P Ni Al S Sb Si
(1) In determining Cu min., Cu may be calculated as Cu + Ni.
(2) Cu + Sum of Named Elements 99.1% min.
Min (%) 70.0 1.5 0.7 20.0
Max (%) 74.0 3.8 2.0 27.0 0.6 0.02 1.0 0.005 0.05 0.20 0.05
Mechanical Properties *
Form Temper Temper Code Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 500 kg load Compressive Strength .001 in. set/in.
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
* Measured at room temperature, 68°F (20°C).
As Centrifugal Cast As Centrifugal Cast M02 35 Min for Standard
35 Min for Standard
12 Min for Standard
25 Min for Standard
As Sand Cast As Sand Cast M01 35 Min for Standard
35 Min for Standard
38 Typ
12 Min for Standard
13 Typ
25 Min for Standard
35 Typ
45 Typ
9 Typ 30 Typ
Castings Not Applicable NA 38 Typ
13 Typ
35 Typ
Physical Properties
Melting Point - Liquidus°F 1725
Melting Point - Solidus°F 1700
Densitylb/cu in. at 68°F 0.307
Specific Gravity 8.5
Electrical Conductivity% IACS at 68°F 18
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F 48.5
Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) 11.5
Specific Heat CapacityBtu/ lb /°F at 68°F 0.09
Modulus of Elasticity in Tensionksi 11000
Casting Characteristics
Casting Attribute Level
Casting Yield High
Drossing High
Effect of Section Size Low
Fluidity Low
Gassing Low
Patternmakers Shrinkage inches per inch 3/16
Shrinkage in Solidification Medium
Fabrication Properties
Technique Suitability
Soldering Excellent
Brazing Fair
Oxyacetylene Welding Fair
Gas Shielded Arc Welding Not Recommended
Coated Metal Arc Welding Not Recommended
Machinability Rating 80
Common Fabrication Processes

No fabrication process properties for this alloy

Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief 500
Solution Treatment 0
Typical uses
Product Category Product Reason Category Reason
Architecture Ornamental Castings Appearance Pleasing Yellow Color
Ornamental Castings Machining Properties Machinability, Good
Ornamental Castings Machining Properties Polishing Characteristics
Ornamental Castings Mechanical Properties Moderate Strength
Builders Hardware Hardware Appearance Pleasing Yellow Color
Hardware Corrosion Resistance Corrosion Resistance
Hardware Machining Properties Machinability, Good
Hardware Machining Properties Polishing Characteristics
Hardware Mechanical Properties Moderate Strength
Consumer Andirons Appearance Pleasing Yellow Color
Andirons Corrosion Resistance Corrosion Resistance
Andirons Machining Properties Machinability, Good
Andirons Machining Properties Polishing Characteristics
Andirons Mechanical Properties Moderate Strength
Chandeliers Appearance Pleasing Yellow Color
Chandeliers Corrosion Resistance Corrosion Resistance
Chandeliers Machining Properties Machinability, Good
Chandeliers Machining Properties Polishing Characteristics
Chandeliers Mechanical Properties Moderate Strength
Industrial Valves Corrosion Resistance Corrosion Resistance
Valves Machining Properties Machinability, Good
Valves Mechanical Properties Moderate Strength
Plumbing Plumbing Fittings Corrosion Resistance Corrosion Resistance
Plumbing Fittings Machining Properties Machinability, Good
Plumbing Fittings Mechanical Properties Moderate Strength
Plumbing Fixtures Appearance Pleasing Yellow Color
Plumbing Fixtures Corrosion Resistance Corrosion Resistance
Plumbing Fixtures Machining Properties Machinability, Good
Plumbing Fixtures Mechanical Properties Moderate Strength
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No Corrosion Properties Available.