Find suppliers for this alloy
C85400
| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | Ni(3) | Al | Si | |
|
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) Cu + Sum of Named Elements 98.9% min. (3) Ni value includes Co. |
||||||||
| Min (%) | 65.0 | 1.5 | 0.50 | 24.0 | ||||
| Max (%) | 70.0 | 3.8 | 1.5 | 32.0 | 0.7 | 1.0 | 0.35 | 0.05 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Compressive Strength .001 in. set/in. (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
30 Min for Standard 30 Min for Standard |
11 Min for Standard |
20 Min for Standard |
|||
| As Sand Cast | As Sand Cast | M01 |
30 Min for Standard 30 Min for Standard 38 Typ |
11 Min for Standard 13 Typ |
20 Min for Standard 35 Typ |
50 Typ |
9 Typ | 28 Typ |
| Melting Point - Liquidus°F | 1725 |
|---|---|
| Melting Point - Solidus°F | 1700 |
| Densitylb/cu in. at 68°F | 0.305 |
| Specific Gravity | 8.44 |
| Electrical Conductivity% IACS at 68°F | 20 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 50.8 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 11.1 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 12000 |
| Magnetic Permeability | 1 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Medium |
| Drossing | High |
| Effect of Section Size | Low |
| Fluidity | Low |
| Gassing | Low |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Medium |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Poor |
| Coated Metal Arc Welding | Poor |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Architecture | Emblem | Appearance | Pleasing Yellow Color |
| Emblem | Machining Properties | Machinability, Good | |
| Emblem | Machining Properties | Polishing Characteristics | |
| Emblem | Mechanical Properties | Moderate Strength | |
| Ornaments | Appearance | Pleasing Yellow Color | |
| Ornaments | Machining Properties | Machinability, Good | |
| Ornaments | Machining Properties | Polishing Characteristics | |
| Ornaments | Mechanical Properties | Moderate Strength | |
| Builders Hardware | Door Hardware for Prisons | Appearance | Appearance |
| Door Hardware for Prisons | Corrosion Resistance | Corrosion Resistance | |
| Door Hardware for Prisons | Machining Properties | Machinability, Good | |
| Door Hardware for Prisons | Machining Properties | Polishing Characteristics | |
| Door Hardware for Prisons | Mechanical Properties | Moderate Strength | |
| Hardware | Appearance | Pleasing Yellow Color | |
| Hardware | Machining Properties | Machinability, Good | |
| Hardware | Machining Properties | Polishing Characteristics | |
| Hardware | Mechanical Properties | Moderate Strength | |
| Ornamental Fittings | Appearance | Pleasing Yellow Color | |
| Ornamental Fittings | Machining Properties | Machinability, Good | |
| Ornamental Fittings | Machining Properties | Polishing Characteristics | |
| Ornamental Fittings | Mechanical Properties | Moderate Strength | |
| Window Hardware | Appearance | Pleasing Yellow Color | |
| Window Hardware | Corrosion Resistance | Corrosion Resistance | |
| Window Hardware | Machining Properties | Machinability, Good | |
| Window Hardware | Machining Properties | Polishing Characteristics | |
| Window Hardware | Mechanical Properties | Moderate Strength | |
| Consumer | Andirons | Appearance | Pleasing Yellow Color |
| Andirons | Machining Properties | Machinability, Good | |
| Andirons | Machining Properties | Polishing Characteristics | |
| Andirons | Mechanical Properties | Moderate Strength | |
| Chandeliers | Appearance | Pleasing Yellow Color | |
| Chandeliers | Machining Properties | Machinability, Good | |
| Chandeliers | Machining Properties | Polishing Characteristics | |
| Chandeliers | Mechanical Properties | Moderate Strength | |
| Decorative Furniture Legs | Appearance | Pleasing Yellow Color | |
| Decorative Furniture Legs | Machining Properties | Machinability, Good | |
| Decorative Furniture Legs | Machining Properties | Polishing Characteristics | |
| Decorative Furniture Legs | Mechanical Properties | Moderate Strength | |
| Furniture | Appearance | Pleasing Yellow Color | |
| Furniture | Machining Properties | Machinability, Good | |
| Furniture | Machining Properties | Polishing Characteristics | |
| Furniture | Mechanical Properties | Moderate Strength | |
| Musical Instruments | Appearance | Pleasing Yellow Color | |
| Musical Instruments | Corrosion Resistance | Corrosion Resistance | |
| Musical Instruments | Machining Properties | Machinability, Good | |
| Musical Instruments | Machining Properties | Polishing Characteristics | |
| Musical Instruments | Mechanical Properties | Moderate Strength | |
| Industrial | Battery Clamps | Corrosion Resistance | Corrosion Resistance |
| Battery Clamps | Machining Properties | Machinability, Good | |
| Battery Clamps | Mechanical Properties | Moderate Strength | |
| Ferrules | Machining Properties | Machinability, Good | |
| Ferrules | Mechanical Properties | Ductility | |
| Ferrules | Mechanical Properties | Moderate Strength | |
| Ferrules | Pressure Tight | Pressure Tight | |
| Gas Cocks | Corrosion Resistance | Corrosion Resistance | |
| Gas Cocks | Machining Properties | Machinability, Good | |
| Gas Cocks | Mechanical Properties | Moderate Strength | |
| Gas Cocks | Pressure Tight | Pressure Tight | |
| Mechanical Components where Looks are Important | Appearance | Pleasing Yellow Color | |
| Mechanical Components where Looks are Important | Machining Properties | Machinability, Good | |
| Mechanical Components where Looks are Important | Machining Properties | Polishing Characteristics | |
| Mechanical Components where Looks are Important | Mechanical Properties | Moderate Strength | |
| Radiator Fittings | Conductivity (Thermal) | Thermal Conductivity | |
| Radiator Fittings | Machining Properties | Machinability, Good | |
| Radiator Fittings | Mechanical Properties | Moderate Strength | |
| Radiator Fittings | Pressure Tight | Pressure Tight | |
| Valves | Corrosion Resistance | Corrosion Resistance | |
| Valves | Machining Properties | Machinability, Good | |
| Valves | Mechanical Properties | Moderate Strength | |
| Valves | Pressure Tight | Pressure Tight | |
| Marine | Marine Hardware | Appearance | Pleasing Yellow Color |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance | |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Marine Hardware | Machining Properties | Machinability, Good | |
| Marine Hardware | Mechanical Properties | Moderate Strength | |
| Ship Trimmings | Appearance | Pleasing Yellow Color | |
| Ship Trimmings | Corrosion Resistance | Corrosion Resistance | |
| Ship Trimmings | Machining Properties | Machinability, Good | |
| Ship Trimmings | Machining Properties | Polishing Characteristics | |
| Ship Trimmings | Mechanical Properties | Moderate Strength | |
| Plumbing | Plumbing Parts | Corrosion Resistance | Corrosion Resistance |
| Plumbing Parts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Plumbing Parts | Machining Properties | Machinability, Good | |
| Plumbing Parts | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | ||
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| As Continuous Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| As Sand Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | ||
| Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
| Valves |
Corrosion Properties