Find suppliers for this alloy
C85470
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Al | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||||||
| Min (%) | 60.0 | 1.0 | .02 | .10 | |||
| Max (%) | 65.0 | .09 | 4.0 | Rem | .20 | .25 | 1.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| As Sand Cast | As Sand Cast | M01 |
50.3 Typ |
21.8 Typ |
20 Typ |
| Melting Point - Liquidus°F | 1688 |
|---|---|
| Melting Point - Solidus°F | 1652 |
| Densitylb/cu in. at 68°F | 0.303 |
| Specific Gravity | 8.4 |
| Electrical Conductivity% IACS at 68°F | 22 |
Casting Characteristics
Fabrication Properties
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Plumbing | Lead-free defined as Calif. AB 1953 max. .25% lead content | ||
| Potable water valve bodies, faucets, plumbing components |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | ||
| As Continuous Cast | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| As Die Cast | ASTM | B176 | BRASS DIE CASTINGS | ||
| As Permanent Mold Cast | ASTM | B806 | PERMANENT MOLD CASTINGS | ||
| As Sand Cast | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Valves | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties