Find suppliers for this alloy
C85550
| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | Ni(2) | Al | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Includes Co. |
||||||||
| Min (%) | 59.0 | 0.30 | ||||||
| Max (%) | 64.0 | 0.09 | 0.30 | Rem | 0.15 | 0.20 | 0.30 | 1.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Impact Strength (ft-lbs) |
Compressive Yield Strength (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| As Die Cast | As Pressure Die Cast | M04 |
60.9 Min 65.3 Typ 69.6 Max |
25 Typ |
56 Typ |
33.7 Typ |
57 Typ | 199 Typ |
| Melting Point - Liquidus°F | 1661 |
|---|---|
| Melting Point - Solidus°F | 1584 |
| Densitylb/cu in. at 68°F | 0.302 |
| Specific Gravity | 8.36 |
| Electrical Conductivity% IACS at 68°F | 19.13 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 44.1 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 6.94 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.11 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10.17 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 11300 |
| Modulus of Rigidityksi | 3900 |
| Magnetic Permeability | 4.95 |
| Poisson's Ratio | 0.46 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Excellent |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Poor |
| Spot Weld | Poor |
| Seam Weld | Not Recommended |
| Butt Weld | Not Recommended |
| Capacity for Being Cold Worked | Not Recommended |
| Capacity for Being Hot Formed | Good |
| Machinability Rating | 71 |
Common Fabrication Processes
| Treatment | Minimum* | Value* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Stress Relief | 572 | |||
| Annealing | 1328 | |||
Typical Uses