| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | Al | Mn | |
|
(1) Cu + Sum of Named Elements 99.0% min. (2) In determining Cu min., Cu may be calculated as Cu + Ni. |
|||||||
| Min (%) | 66.0 | 2.0 | 4.5 | 2.5 | |||
| Max (%) | 68.0 | 0.20 | 0.20 | Rem | 4.0 | 5.5 | 5.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load | Izod (ft-lbs) |
Compressive Strength .001 in. set/in. (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| As Sand Cast | As Sand Cast | M01 |
95 Typ |
50 Typ |
20 Typ |
180 Typ |
12 Typ | 50 Typ |
| (1)Field Strength 16 kA/m | |
| Melting Point - Liquidus°F | 1725 |
|---|---|
| Melting Point - Solidus°F | 1650 |
| Densitylb/cu in. at 68°F | 0.288 |
| Specific Gravity | 7.97 |
| Electrical Conductivity% IACS at 68°F | 8 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 20.5 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 12 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 15000 |
| Magnetic Permeability | 1.24 (1) |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Low |
| Drossing | High |
| Effect of Section Size | Low |
| Fluidity | Medium |
| Gassing | Low |
| Patternmakers Shrinkage inches per inch | 4/16 |
| Shrinkage in Solidification | High |
| Technique | Suitability |
|---|---|
| Soldering | Poor |
| Brazing | Poor |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Good |
| Machinability Rating | 30 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Consumer | Gun Mounts | Appearance | Appearance |
| Gun Mounts | Corrosion Resistance | Corrosion Resistance | |
| Gun Mounts | Mechanical Properties | Moderate Strength | |
| Industrial | Bearings | Corrosion Resistance | Corrosion Resistance |
| Bearings | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Mechanical Properties | Moderate Strength | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Mechanical Properties | Moderate Strength | |
| Gears | Corrosion Resistance | Corrosion Resistance | |
| Gears | Friction & Wear Properties | Wear Resistance | |
| Gears | Machining Properties | Machinability, Good | |
| Gears | Mechanical Properties | Moderate Strength | |
| Gun Mounts | Appearance | Appearance | |
| Gun Mounts | Corrosion Resistance | Corrosion Resistance | |
| Gun Mounts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Gun Mounts | Friction & Wear Properties | Wear Resistance | |
| Gun Mounts | Mechanical Properties | Moderate Strength | |
| Marine | Marine Castings | Corrosion Resistance | Corrosion Resistance |
| Marine Castings | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Marine Castings | Mechanical Properties | Ductility | |
| Marine Castings | Mechanical Properties | Moderate Strength | |
| Marine Racing Propellers | Corrosion Resistance | Corrosion Resistance | |
| Marine Racing Propellers | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Marine Racing Propellers | Corrosion Resistance | Corrosion Resistance to the Atmosphere | |
| Marine Racing Propellers | Friction & Wear Properties | Wear Resistance | |
| Marine Racing Propellers | Mechanical Properties | Moderate Strength |
Applicable Specifications
Corrosion Properties