Chemical Composition
Element
Cu(1,2)PbSnZnFeNi(3)AlMn
(1) Cu + Sum of Named Elements 99.0% min. (2) In determining Cu min., Cu may be calculated as Cu + Ni. (3) Ni value includes Co.
Min (%)60.022.02.03.02.5
Max (%)66.00.200.2028.04.01.04.95.0
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 3000 kg load
Izod
(ft-lbs)
Compressive Strength .001 in. set/in.
(ksi)
As Centrifugal CastAs Centrifugal CastM0290   Min for Standard
45   Min for Standard
18   Min for Standard
As Continuous CastAs Continuous CastM0790   Min for Standard
45   Min for Standard
18   Min for Standard
As Sand CastAs Sand CastM0190   Min for Standard
95   Typ
45   Min for Standard
48   Typ
18   Min for Standard
20   Typ
180   Typ
12   Typ
50   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) Field Strength 16 kA/m
Melting Point - Liquidus°F1725
Melting Point - Solidus°F1650
Densitylb/cu in. at 68°F0.288
Specific Gravity7.97
Electrical Conductivity% IACS at 68°F8
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F20.5
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)12
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Magnetic Permeability1.24(1)
Casting Characteristics
Casting Attribute Level
Casting YieldLow
DrossingHigh
Effect of Section SizeLow
FluidityMedium
GassingLow
Patternmakers Shrinkageinches per inch4/16
Shrinkage in SolidificationHigh
Fabrication Properties
Technique Suitability
SolderingPoor
BrazingPoor
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingGood
Machinability Rating30
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief500
Solution Treatment0
Typical uses
Product Category Product Reason Category Reason
Builders HardwareBracketsCorrosion ResistanceCorrosion Resistance
BracketsMechanical PropertiesModerate Strength
Structural PartsCorrosion ResistanceCorrosion Resistance
Structural PartsMechanical PropertiesModerate Strength
FastenersScrew Down NutsCorrosion ResistanceCorrosion Resistance
Screw Down NutsFriction & Wear PropertiesWear Resistance
Screw Down NutsMechanical PropertiesModerate Strength
IndustrialBushingsCorrosion ResistanceCorrosion Resistance
BushingsFriction & Wear PropertiesWear Resistance
BushingsMechanical PropertiesModerate Strength
CamsCorrosion ResistanceCorrosion Resistance
CamsFriction & Wear PropertiesWear Resistance
CamsMechanical PropertiesModerate Strength
FramesCorrosion ResistanceCorrosion Resistance
FramesFriction & Wear PropertiesWear Resistance
FramesMechanical PropertiesModerate Strength
GearsCorrosion ResistanceCorrosion Resistance
GearsFriction & Wear PropertiesWear Resistance
GearsMechanical PropertiesModerate Strength
High Strength Machine PartsConductivity (Thermal)Thermal Conductivity
High Strength Machine PartsCorrosion ResistanceCorrosion Resistance
High Strength Machine PartsCorrosion ResistanceCorrosion Resistance to the Atmosphere
High Strength Machine PartsFriction & Wear PropertiesWear Resistance
High Strength Machine PartsMechanical PropertiesModerate Strength
HooksCorrosion ResistanceCorrosion Resistance
HooksMechanical PropertiesModerate Strength
Marine Racing PropellersCorrosion ResistanceCorrosion Resistance
Marine Racing PropellersCorrosion ResistanceCorrosion Resistance to Salt Water
Marine Racing PropellersCorrosion ResistanceCorrosion Resistance to the Atmosphere
Marine Racing PropellersFriction & Wear PropertiesWear Resistance
Marine Racing PropellersMechanical PropertiesModerate Strength
Pressing Dies for Wood PulpCorrosion ResistanceCorrosion Resistance
Pressing Dies for Wood PulpFriction & Wear PropertiesWear Resistance
Pressing Dies for Wood PulpMechanical PropertiesModerate Strength
ShaftsCorrosion ResistanceCorrosion Resistance
ShaftsFriction & Wear PropertiesWear Resistance
ShaftsMechanical PropertiesModerate Strength
StrutsCorrosion ResistanceCorrosion Resistance
StrutsCorrosion ResistanceCorrosion Resistance to the Atmosphere
StrutsFriction & Wear PropertiesWear Resistance
StrutsMechanical PropertiesModerate Strength
Valve StemsCorrosion ResistanceCorrosion Resistance
Valve StemsFriction & Wear PropertiesWear Resistance
Valve StemsMechanical PropertiesModerate Strength
Wear Rings for Pressing Dies for Wood Pulp IndustryCorrosion ResistanceCorrosion Resistance
Wear Rings for Pressing Dies for Wood Pulp IndustryFriction & Wear PropertiesWear Resistance
Wear Rings for Pressing Dies for Wood Pulp IndustryMechanical PropertiesModerate Strength
Worm GearsCorrosion ResistanceCorrosion Resistance
Worm GearsFriction & Wear PropertiesWear Resistance
Worm GearsMechanical PropertiesModerate Strength
MarineBoat PartsCorrosion ResistanceCorrosion Resistance
Boat PartsCorrosion ResistanceCorrosion Resistance to Salt Water
Boat PartsCorrosion ResistanceCorrosion Resistance to the Atmosphere
Boat PartsFriction & Wear PropertiesWear Resistance
Boat PartsMechanical PropertiesModerate Strength
ClampsCorrosion ResistanceCorrosion Resistance
ClampsCorrosion ResistanceCorrosion Resistance to Salt Water
ClampsMechanical PropertiesModerate Strength
Marine CastingsCorrosion ResistanceCorrosion Resistance
Marine CastingsCorrosion ResistanceCorrosion Resistance to Salt Water
Marine CastingsCorrosion ResistanceCorrosion Resistance to the Atmosphere
Marine CastingsFriction & Wear PropertiesWear Resistance
Marine CastingsMechanical PropertiesModerate Strength
RuddersCorrosion ResistanceCorrosion Resistance
RuddersCorrosion ResistanceCorrosion Resistance to Salt Water
RuddersCorrosion ResistanceCorrosion Resistance to the Atmosphere
RuddersFriction & Wear PropertiesWear Resistance
RuddersMechanical PropertiesModerate Strength
OrdnanceGun MountsAppearanceAppearance
Gun MountsCorrosion ResistanceCorrosion Resistance
Gun MountsFriction & Wear PropertiesWear Resistance
Gun MountsMechanical PropertiesModerate Strength
Applicable Specifications
Form Sub-Form System Standard Description
As Centrifugal CastCastingsASTMB271/B271MCOPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Continuous CastCastingsASTMB505/B505MCOPPER BASE ALLOY CONTINUOUS CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Sand CastCastingsASTMB584COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
CastingsASTMB763/B763MCOPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
Ingot
ASTMB30COPPER BASE ALLOYS IN INGOT FORM
FEDERALQQ-C-523COPPER ALLOY INGOTS: BRASS (YELLOW HIGH STRENGTH) MANGANESE AND MANGANESE-ALUMINUM BRONZE
Precision CastCastingsMILITARYMIL-C-11866CASTINGS, PRECISION, NONFERROUS
Valves
Corrosion Properties

No information available.