C86350
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | Ni(2) | Al | Mg | Mn | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
|||||||||
| Min (%) | 60.0 | 0.30 | 2.0 | ||||||
| Max (%) | 64.0 | 0.09 | 0.8 | Rem | 1.0 | 0.50 | 1.1 | 0.10 | 5.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
Shear Strength (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Castings | As Sand Cast | M01 |
52.2 Min 58 Typ 63.8 Max |
31.9 Typ |
348 Typ |
| Melting Point - Liquidus°F | 16900 |
|---|---|
| Melting Point - Solidus°F | 1600 |
| Densitylb/cu in. at 68°F | 0.296 |
| Specific Gravity | 8.203 |
| Electrical Conductivity% IACS at 68°F | 8.52 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 21.6 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.17 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 10.9 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11.2 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.098 |
| Modulus of Elasticity in Tensionksi | 15300 |
| Modulus of Rigidityksi | 5400 |
| Poisson's Ratio | 0.42 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Fair |
| Seam Weld | Fair |
| Butt Weld | Fair |
| Capacity for Being Cold Worked | Not Recommended |
| Capacity for Being Hot Formed | Good |
| Machinability Rating | 65 |
Common Fabrication Processes
| Treatment | Minimum* | Value* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Stress Relief | 572 | |||
| Annealing | 1328 | |||
Typical Uses
Applicable Specifications
Corrosion Properties