Find suppliers for this alloyC86350
Chemical Composition
Element
Cu(1)PbSnZnFeNi(2)AlMgMn
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co.
Min (%)60.00.302.0
Max (%)64.00.090.8Rem1.00.501.10.105.0
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
Shear Strength
(ksi)
Impact Strength
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
CastingsAs Sand CastM0152.2   Min
58   Typ
63.8   Max
31.9   Typ
  Typ
348   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F16900
Melting Point - Solidus°F1600
Densitylb/cu in. at 68°F0.296
Specific Gravity8.203
Electrical Conductivity% IACS at 68°F8.52
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F21.6
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)9.17
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)10.9
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.2
Specific Heat CapacityBtu/ lb /°F at 68°F0.098
Modulus of Elasticity in Tensionksi15300
Modulus of Rigidityksi5400
Poisson's Ratio0.42
Casting Characteristics

No casting characteristics for this alloy

Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingFair
Spot WeldFair
Seam WeldFair
Butt WeldFair
Capacity for Being Cold WorkedNot Recommended
Capacity for Being Hot FormedGood
Machinability Rating65
Fabrication Process Properties

No fabrication process properties for this alloy

    
Thermal Properties
Treatment Minimum* Value*
* Temperature is measured in Fahrenheit.
Stress Relief572
Annealing1328
Typical uses
Product Category Product Reason Category Reason
PlumbingValve Bodies, Faucets, Plumbing Components
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties