Find suppliers for this alloy
C86550
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | Ni(3) | Al | Mn | Si | |
|
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) Cu + Sum of Named Elements 99.0% min. (3) Ni value includes Co. |
|||||||||
| Min (%) | 57.0 | 0.7 | 0.50 | 0.10 | |||||
| Max (%) | 0.50 | 1.0 | Rem | 2.0 | 1.0 | 2.5 | 3.0 | 0.10 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load | Compressive Strength .001 in. set/in. (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
Fatigue Strength** (ksi) |
|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||
| As Sand Cast | As Sand Cast | M01 |
47 Min |
17 Min |
18 Min |
100 Min |
16 Typ | 61 Typ | 14 Typ |
| Densitylb/cu in. at 68°F | 0.3 |
|---|---|
| Specific Gravity | 8.3 |
| Electrical Conductivity% IACS at 68°F | 22 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 50 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 11.4 |
| Modulus of Elasticity in Tensionksi | 14000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Low |
| Drossing | Low |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 5/32 |
| Shrinkage in Solidification | High |
| Technique | Suitability |
|---|---|
| Soldering | Fair |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Fair |
| Machinability Rating | 15 |
Common Fabrication Processes
| Treatment | Time** | |||
|---|---|---|---|---|
| ** Time is measured in minutes. | ||||
| Solution Treatment | 0 | |||
Typical Uses
Applicable Specifications
Corrosion Properties