Find suppliers for this alloyC86700
Element | ||||||||
---|---|---|---|---|---|---|---|---|
Cu(1,2) | Pb | Sn | Zn | Fe | Ni(3) | Al | Mn | |
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) Cu + Sum of Named Elements 99.0% min. (3) Ni value includes Co. | ||||||||
Min (%) | 55.0 | 0.50 | 30.0 | 1.0 | 1.0 | 0.10 | ||
Max (%) | 60.0 | 1.5 | 1.5 | 38.0 | 3.0 | 1.0 | 3.0 | 3.5 |
Form | Temper | Temper Code | Tensile Strength (ksi) | YS-0.5% Ext (ksi) | Elongation (%) | Rockwell B scale | Brinell Hardness, 3000 kg load | ||
---|---|---|---|---|---|---|---|---|---|
As Centrifugal Cast | As Centrifugal Cast | M02 | 80 Min for Standard | 32 Min for Standard | 15 Min for Standard | ||||
As Sand Cast | As Sand Cast | M01 | 80 Min for Standard 85 Typ | 32 Min for Standard 42 Typ | 15 Min for Standard 20 Typ | 80 Typ | 155 Typ | ||
* Measured at room temperature, 68°F (20°C). |
Melting Point - Liquidus°F | 1616 |
---|---|
Melting Point - Solidus°F | 1583 |
Densitylb/cu in. at 68°F | 0.301 |
Specific Gravity | 8.33 |
Electrical Conductivity% IACS at 68°F | 17 |
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F) | 11 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
Modulus of Elasticity in Tensionksi | 15000 |
Casting Attribute | Level |
---|---|
Casting Yield | Low |
Drossing | High |
Effect of Section Size | Low |
Fluidity | Medium |
Gassing | Low |
Patternmakers Shrinkageinches per inch | 4/16 |
Shrinkage in Solidification | High |
Technique | Suitability |
---|---|
Soldering | Fair |
Brazing | Fair |
Oxyacetylene Welding | Poor |
Gas Shielded Arc Welding | Poor |
Coated Metal Arc Welding | Poor |
Machinability Rating | 55 |
Common Fabrication Processes
- Casting
Treatment | Value* | Time** | |||
---|---|---|---|---|---|
* Temperature is measured in Fahrenheit. ** Time is measured in minutes. | |||||
Stress Relief | 500 | ||||
Solution Treatment | 0 |
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Builders Hardware | Brackets | Corrosion Resistance | Corrosion Resistance |
Brackets | Machining Properties | Machinability, Good | |
Brackets | Mechanical Properties | High Strength | |
Fasteners | Screw Down Nuts | Corrosion Resistance | Corrosion Resistance |
Screw Down Nuts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Screw Down Nuts | Friction & Wear Properties | Wear Resistance | |
Screw Down Nuts | Machining Properties | Machinability, Good | |
Screw Down Nuts | Mechanical Properties | High Strength | |
Industrial | Bearings | Corrosion Resistance | Corrosion Resistance |
Bearings | Mechanical Properties | High Strength | |
Cams | Corrosion Resistance | Corrosion Resistance | |
Cams | Friction & Wear Properties | Wear Resistance | |
Cams | Machining Properties | Machinability, Good | |
Cams | Mechanical Properties | High Strength | |
Fittings | Corrosion Resistance | Corrosion Resistance | |
Fittings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Fittings | Friction & Wear Properties | Wear Resistance | |
Fittings | Machining Properties | Machinability, Good | |
Fittings | Mechanical Properties | High Strength | |
Lever Arms | Corrosion Resistance | Corrosion Resistance | |
Lever Arms | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Lever Arms | Friction & Wear Properties | Wear Resistance | |
Lever Arms | Machining Properties | Machinability, Good | |
Lever Arms | Mechanical Properties | High Strength | |
Machinery Parts | Corrosion Resistance | Corrosion Resistance | |
Machinery Parts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Machinery Parts | Friction & Wear Properties | Wear Resistance | |
Machinery Parts | Machining Properties | Machinability, Good | |
Machinery Parts | Mechanical Properties | High Strength | |
Moderate Duty Gears | Corrosion Resistance | Corrosion Resistance | |
Moderate Duty Gears | Friction & Wear Properties | Wear Resistance | |
Moderate Duty Gears | Machining Properties | Machinability, Good | |
Moderate Duty Gears | Mechanical Properties | High Strength | |
Propellers | Corrosion Resistance | Corrosion Resistance | |
Propellers | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Propellers | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Propellers | Friction & Wear Properties | Wear Resistance | |
Propellers | Machining Properties | Machinability, Good | |
Propellers | Mechanical Properties | High Strength | |
Valve Stems | Corrosion Resistance | Corrosion Resistance | |
Valve Stems | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Valve Stems | Friction & Wear Properties | Wear Resistance | |
Valve Stems | Machining Properties | Machinability, Good | |
Valve Stems | Mechanical Properties | High Strength | |
Marine | Marine Hardware | Corrosion Resistance | Corrosion Resistance |
Marine Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Marine Hardware | Friction & Wear Properties | Wear Resistance | |
Marine Hardware | Machining Properties | Machinability, Good | |
Marine Hardware | Mechanical Properties | High Strength | |
Propellers | Corrosion Resistance | Corrosion Resistance | |
Propellers | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Propellers | Mechanical Properties | Ductility | |
Propellers | Mechanical Properties | High Strength |
Form | Sub-Form | System | Standard | Description |
---|---|---|---|---|
As Centrifugal Cast | Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS |
As Sand Cast | Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS |
Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | |
Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties