Find suppliers for this alloyC86800
Chemical Composition
Element
Cu(1,2)PbSnZnFeNi(3)AlMn
(1) Cu + Sum of Named Elements 99.0% min. (2) In determining Cu min., Cu may be calculated as Cu + Ni. (3) Ni value includes Co.
Min (%)53.51.02.52.5
Max (%)57.00.201.0Rem2.54.02.04.0
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 3000 kg load
As Sand CastAs Sand CastM0182   Typ
38   Typ
22   Typ
80   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1652
Melting Point - Solidus°F1616
Densitylb/cu in. at 68°F0.29
Specific Gravity8.03
Electrical Conductivity% IACS at 68°F9
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Casting Characteristics

No casting characteristics for this alloy

Fabrication Properties
Technique Suitability
SolderingFair
BrazingFair
Oxyacetylene WeldingPoor
Gas Shielded Arc WeldingPoor
Coated Metal Arc WeldingPoor
Machinability Rating30
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief500
Solution Treatment0
Typical uses
Product Category Product Reason Category Reason
IndustrialFittingsCorrosion ResistanceCorrosion Resistance
FittingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
FittingsMechanical PropertiesDuctility
FittingsMechanical PropertiesHigh Strength
PropellersCorrosion ResistanceCorrosion Resistance
PropellersCorrosion ResistanceCorrosion Resistance to Numerous Environments
PropellersCorrosion ResistanceCorrosion Resistance to Salt Water
PropellersMechanical PropertiesDuctility
PropellersMechanical PropertiesHigh Strength
Applicable Specifications
Form
Valves
Corrosion Properties

No information available.