Chemical Composition
Elements
Cu(1) Pb Zn Al Si
(1) Cu + Sum of Named Elements 99.5% min.
Min (%) 79.0 12.0 3.0
Max (%) 0.09 16.0 0.50 5.0
Mechanical Properties *
Form Temper Temper Code Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 500 kg load Brinell Hardness, 3000 kg load Stress Rupture
(ksi)
Charpy V-Notch Impact Strength
(ft-lbs)
Compressive Strength .001 in. set/in.
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
Creep Strength (0.1% per 10,000 hours)
(ksi)
Fatigue Strength**
(ksi)
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
As Centrifugal Cast As Centrifugal Cast M02 60 Min for Standard
24 Min for Standard
16 Min for Standard
As Permanent Mold Cast As Permanent Mold Cast M05 80 Min for Standard
30 Min for Standard
15 Min for Standard
As Sand Cast As Sand Cast M01 60 Min for Standard
67 Typ
24 Min for Standard
30 Typ
16 Min for Standard
21 Typ
115 Typ
134 Typ
18 Typ 32 Typ
27 Typ 75 Typ 11 Typ 22 Typ
Physical Properties
Melting Point - Liquidus°F 1680
Melting Point - Solidus°F 1510
Densitylb/cu in. at 68°F 0.299
Specific Gravity 8.28
Electrical Conductivity% IACS at 68°F 6.7
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F 16
Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) 10.9
Specific Heat CapacityBtu/ lb /°F at 68°F 0.09
Modulus of Elasticity in Tensionksi 15400
Casting Characteristics
Casting Attribute Level
Casting Yield Medium
Drossing Low
Effect of Section Size Medium
Fluidity High
Gassing Medium
Patternmakers Shrinkage inches per inch 3/16
Shrinkage in Solidification Medium
Fabrication Properties
Technique Suitability
Soldering Excellent
Brazing Excellent
Oxyacetylene Welding Fair
Gas Shielded Arc Welding Excellent
Coated Metal Arc Welding Not Recommended
Spot Weld Good
Seam Weld Good
Butt Weld Good
Machinability Rating 50
Common Fabrication Processes

No fabrication process properties for this alloy

Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief 500
Solution Treatment 0
Typical uses
Product Category Product Reason Category Reason
Builders Hardware Window Hardware Appearance Appearance
Window Hardware Casting Characteristics Castability
Window Hardware Corrosion Resistance Corrosion Resistance
Window Hardware Mechanical Properties High Strength
Industrial Bearings Corrosion Resistance Corrosion Resistance
Bearings Mechanical Properties Ductility
Bearings Mechanical Properties High Strength
Fittings Casting Characteristics Castability
Fittings Corrosion Resistance Corrosion Resistance
Fittings Mechanical Properties High Strength
Gears Corrosion Resistance Corrosion Resistance
Gears Mechanical Properties Ductility
Gears Mechanical Properties High Strength
Impellers Corrosion Resistance Corrosion Resistance
Impellers Corrosion Resistance Resists Stress Corrosion Cracking in Marine Environments
Impellers Mechanical Properties Ductility
Impellers Mechanical Properties High Strength
Levers Casting Characteristics Castability
Levers Corrosion Resistance Corrosion Resistance
Levers Mechanical Properties High Strength
Pump Fixtures Casting Characteristics Castability
Pump Fixtures Corrosion Resistance Corrosion Resistance
Pump Fixtures Corrosion Resistance Corrosion Resistance to Fresh Water
Pump Fixtures Corrosion Resistance Corrosion Resistance to Numerous Environments
Pump Fixtures Corrosion Resistance Corrosion Resistance to Salt Water
Pump Fixtures Mechanical Properties High Strength
Valve Bodies Casting Characteristics Castability
Valve Bodies Corrosion Resistance Corrosion Resistance
Valve Bodies Mechanical Properties High Strength
Marine Boat Parts Casting Characteristics Castability
Boat Parts Corrosion Resistance Corrosion Resistance
Boat Parts Corrosion Resistance Corrosion Resistance to Salt Water
Boat Parts Mechanical Properties High Strength
Small Boat Propellers Corrosion Resistance Corrosion Resistance
Small Boat Propellers Corrosion Resistance Corrosion Resistance to Salt Water
Small Boat Propellers Corrosion Resistance Resists Stress Corrosion Cracking in Marine Environments
Small Boat Propellers Mechanical Properties Ductility
Small Boat Propellers Mechanical Properties High Strength
Plumbing Fixtures Casting Characteristics Castability
Fixtures Corrosion Resistance Corrosion Resistance
Fixtures Mechanical Properties High Strength
Fixtures Mechanical Properties Retains Strength at Elevated Temperatures
Applicable Specifications
Form Specific Sub-Form Application System Standard Description
As Centrifugal Cast Castings SAE J462 CAST COPPER ALLOYS
Castings SAE J461 WROUGHT AND CAST COPPER ALLOYS
Castings ASTM B271/B271M COPPER BASE ALLOY CENTRIFUGAL CASTINGS
As Permanent Mold Cast Castings ASTM B806 PERMANENT MOLD CASTINGS
As Sand Cast Castings ASTM B763/B763M COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
Castings ASTM B584 COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
Ingot ASTM B30 COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties