Find suppliers for this alloy
C87700
| Elements | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni | Mn | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.2% min. |
||||||||||
| Min (%) | 87.5 | 7.0 | 2.5 | |||||||
| Max (%) | 0.09 | 2.0 | 9.0 | 0.50 | 0.15 | 0.25 | 0.8 | 0.10 | 3.5 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| As Continuous Cast | As Continuous Cast | M07 |
29.0 Min 43.5 Typ 58 Max |
11.6 Min 17.4 Typ 23.2 Max |
3.6 Typ |
11.6 Typ |
| Forgings | As Hot Forged - Air Cooled | M10 |
29 Min 43.5 Typ 58 Max |
11.6 Min 17.4 Typ 23.2 Max |
3.6 Typ |
11.6 Typ |
| Melting Point - Liquidus°F | 1796 |
|---|---|
| Melting Point - Solidus°F | 1652 |
| Densitylb/cu in. at 68°F | 0.311 |
| Specific Gravity | 8.5 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Fair |
| Brazing | Fair |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Fair |
| Capacity for Being Hot Formed | Good |
| Forgeability Rating | 80 |
| Machinability Rating | 70 |
Common Fabrication Processes
Thermal Properties
Typical Uses
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Continuous Cast | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| Die Forging | ASTM | B283/B283M | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
| Rod, Bar & Shapes | Forgings | ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES |
Corrosion Properties