Find suppliers for this alloyC87860
Element | ||||||||||
---|---|---|---|---|---|---|---|---|---|---|
Cu(1) | Pb | Sn | Zn | Fe | P | Ni(2) | Mn | Si | Zr | |
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. | ||||||||||
Min (%) | 75.0 | .05 | 2.7 | .002 | ||||||
Max (%) | 79.0 | .09 | .30 | Rem | .10 | .20 | .20 | .10 | 3.5 | .030 |
Form | Temper | Temper Code | Tensile Strength (ksi) | YS-0.2% Offset | Elongation (%) | Rockwell B scale | ||
---|---|---|---|---|---|---|---|---|
As Sand Cast | As Sand Cast | M01 | 55.1 Min 65.3 Typ | 20.3 Min 26.1 Typ | 15 Min | 60 Typ | ||
Permanent Mold Castings | As Permanent Mold Cast | M05 | 62.4 Min 72.5 Typ | 23.2 Min 29 Typ | 15 Min | 65 Typ | ||
* Measured at room temperature, 68°F (20°C). |
Melting Point - Liquidus°F | 1643 |
---|---|
Melting Point - Solidus°F | 1571 |
Densitylb/cu in. at 68°F | 0.3 |
Specific Gravity | 8.3 |
Electrical Conductivity% IACS at 68°F | 8 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 21.7 |
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F) | 10.3 |
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F) | 10.3 |
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F) | 10.4 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
Modulus of Elasticity in Tensionksi | 15200 |
Poisson's Ratio | 0.33 |
Casting Characteristics
Technique | Suitability |
---|---|
Soldering | Excellent |
Brazing | Good |
Oxyacetylene Welding | Good |
Gas Shielded Arc Welding | Good |
Coated Metal Arc Welding | Good |
Spot Weld | Good |
Seam Weld | Good |
Butt Weld | Good |
Capacity for Being Cold Worked | Poor |
Capacity for Being Hot Formed | Excellent |
Forgeability Rating | 95 |
Machinability Rating | 70 |
Fabrication Process Properties
Treatment | Minimum* | Maximum* | |||
---|---|---|---|---|---|
* Temperature is measured in Fahrenheit. | |||||
Annealing | 932 | 1112 |
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Industrial | Bolts | ||
Nuts | |||
Plumbing | Lead-free defined as Calif. AB 1953 max. .25% lead content | ||
Potable Water Components, Valves, Pump Components , Plumbing Fittings, Meter Cases |
Applicable Specifications
Corrosion Properties