Find suppliers for this alloyC89520
Chemical Composition
Element
Cu(1)PbSnZnFeNi(2)AlBi(3)SSbSe(4)
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. (3) Bi:Se >= 2:1 (4) Bi:Se >= 2:1
Min (%)85.05.04.01.60.8
Max (%)87.00.096.06.00.201.00.0052.20.080.251.1
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 500 kg load
As Sand CastAs Sand CastM0131   Typ
21   Typ
10   Typ
54   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1842
Melting Point - Solidus°F353
Casting Characteristics
Casting Attribute Level
Casting YieldHigh
DrossingMedium
Effect of Section SizeLow
FluidityMedium
GassingMedium
Shrinkage in SolidificationMedium
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingNot Recommended
Coated Metal Arc WeldingNot Recommended
Machinability Rating85
Common Fabrication Processes
  • Casting
Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
PlumbingPlumbing CastingsCorrosion ResistanceCorrosion Resistance
Plumbing CastingsLead FreeLead Free
Plumbing CastingsMachining PropertiesMachinability, Good
Plumbing CastingsMechanical PropertiesModerate Strength
Applicable Specifications
Form System Standard Description
As Sand CastASTMB584COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
IngotASTMB30COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties