Find suppliers for this alloy
C89530
| Elements | ||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni(2) | Al | Bi | Sb | Si | Se | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
||||||||||||
| Min (%) | 84.0 | 3.5 | 7.0 | 1.0 | 0.10 | |||||||
| Max (%) | 89.0 | 0.20 | 6.0 | 9.0 | 0.30 | 0.05 | 1.0 | 0.01 | 2.0 | 0.20 | 0.01 | 0.30 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load | Shear Strength (ksi) |
Impact Strength (ft-lbs) |
Compressive Yield Strength (ksi) |
Fatigue Strength** (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||
| As Sand Cast | As Sand Cast | M01 |
28.3 Min 33.4 Typ 38 Max |
13.1 Min 15.2 Typ 19 Max |
15 Min |
52 Typ |
1.8 Typ |
5.3 Typ | 247 Typ | 10.2 Typ |
Physical Properties
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Not Recommended |
| Capacity for Being Cold Worked | Poor |
| Capacity for Being Hot Formed | Poor |
| Machinability Rating | 84 |
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Plumbing | Cu based devices for lead-free water applications, | ||
| Lead-free defined as Calif. AB 1953 max. .25% lead content | |||
| Lead-free, dezincification resistant for potable water components | |||
| valves, fittings, pumps, meters |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Sand Cast | Valves | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | |
| ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | |||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties