Find suppliers for this alloy
C89535
| Elements | ||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni(2) | Al | Bi | Sb | Si | Se | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
||||||||||||
| Min (%) | 84.0 | 2.5 | 5.0 | 0.30 | 0.8 | |||||||
| Max (%) | 89.0 | 0.25 | 5.5 | 9.0 | 0.30 | 0.40 | 1.0 | 0.01 | 2.0 | 0.20 | 0.01 | 0.50 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Compressive Yield Strength (ksi) |
Fatigue Strength** (ksi) |
|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||
| As Sand Cast | As Sand Cast | M01 |
32 Min 38 Typ 44.3 Max |
16 Min 19 Typ 22 Max |
15 Min |
52 Min |
30 Min |
232 Min |
13 Min |
| Melting Point - Liquidus°F | 1886 |
|---|---|
| Melting Point - Solidus°F | 1472 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.79 |
| Electrical Conductivity% IACS at 68°F | 16.9 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 40.6 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.4 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.7 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 14170 |
| Modulus of Rigidityksi | 5110 |
| Magnetic Permeability | 1 |
| Poisson's Ratio | 0.36 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Fair |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Not Recommended |
| Capacity for Being Cold Worked | Poor |
| Capacity for Being Hot Formed | Poor |
| Machinability Rating | 75 |
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Plumbing | Cu Alloy based devices for lead-free water applications | ||
| Lead-free defined as Calif. AB 1953 max. .25% lead content | |||
| Lead-free, dezinfication resistant alloy for potable water components | |||
| valves, fittings, pumps, meters |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Sand Cast | Valves | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | |
| ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | |||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties