Find suppliers for this alloyC89550
Chemical Composition
Element
Cu(1)PbSnZnFePNi(2)AlBiSSbSiSe
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co.
Min (%)58.00.0032.00.100.60.01
Max (%)64.00.091.238.00.500.011.00.61.20.050.050.250.10
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
As Sand CastAs Sand CastM0135   Min
48   Typ
20   Min
28   Typ
21   Min
29   Typ
5   Min
8   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1638
Melting Point - Solidus°F1588
Casting Characteristics

No casting characteristics for this alloy

Fabrication Properties
Technique Suitability Footnote
SolderingGood
BrazingGood
Machinability Rating971.0% Bi
Machinability Rating750.7% Bi
Common Fabrication Processes
  • Casting
Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
PlumbingPlumbing CastingsLead FreeLead Free
Plumbing CastingsMechanical PropertiesModerate Strength
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.