| Elements | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | P | Al | B | Bi | Mn | Sb | |
|
(1) Cu + Sum of Named Elements 99.8% min. |
||||||||||
| Min (%) | 61.5 | 0.50 | 0.15 | 0.15 | 0.002 | 0.15 | 0.20 | 0.25 | ||
| Max (%) | 62.5 | 0.10 | 0.6 | Rem | 0.20 | 0.25 | 0.005 | 0.30 | 0.40 | 0.35 |
| Form | Temper | Temper Code | YS-0.2% Offset (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load | Shear Strength (ksi) |
Compressive Yield Strength (ksi) |
Ultimate Tensile Strength in Shear (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| As Permanent Mold Cast | As Permanent Mold Cast | M05 | 22.5 Typ |
39 Typ |
73 Typ |
35.8 Typ |
374.5 Typ | 52.6 Typ |
| Melting Point - Liquidus°F | 1697 |
|---|---|
| Melting Point - Solidus°F | 1638 |
| Densitylb/cu in. at 68°F | 0.304 |
| Specific Gravity | 8.42 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 54.9 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11.5 |
| Modulus of Elasticity in Tensionksi | 14240 |
| Poisson's Ratio | 0.301 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Fluidity | High |
| Gassing | Low |
| Shrinkage in Solidification | Medium |
| Technique | Suitability |
|---|---|
| Forgeability Rating | 95 |
| Machinability Rating | 85 |