Find suppliers for this alloy
C89833
| Elements | ||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni(2) | Al | Bi | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.3% min. (2) Ni value includes Co. |
||||||||||||
| Min (%) | 86.0 | 4.0 | 2.0 | 1.7 | ||||||||
| Max (%) | 91.0 | 0.09 | 6.0 | 6.0 | 0.30 | 0.050 | 1.0 | 0.005 | 2.7 | 0.08 | 0.25 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Izod (ft-lbs) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| As Sand Cast | As Sand Cast | M01 |
37 Typ |
17 Typ |
28 Typ |
60 Typ |
12 Typ |
| Melting Point - Liquidus°F | 1877 |
|---|---|
| Melting Point - Solidus°F | 1454 |
| Densitylb/cu in. at 68°F | 0.317 |
| Specific Gravity | 8.78 |
| Electrical Conductivity% IACS at 68°F | 17.8 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 41 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 13 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.085 |
| Modulus of Elasticity in Tensionksi | 15500 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | Low |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 11/64 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Poor |
| Machinability Rating | 81 |
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Corrosion Resistant, Pressure Tight Castings | Corrosion Resistance | Corrosion Resistance |
| Corrosion Resistant, Pressure Tight Castings | Friction & Wear Properties | Wear Resistance | |
| Corrosion Resistant, Pressure Tight Castings | Lead-Free | Lead-Free Alternative to Leaded Alloy C83600 | |
| Corrosion Resistant, Pressure Tight Castings | Mechanical Properties | Moderate Strength | |
| Impellers | Corrosion Resistance | Corrosion Resistance | |
| Impellers | Friction & Wear Properties | Wear Resistance | |
| Impellers | Lead Free | Lead-Free Alternative to Leaded Alloy C83600 | |
| Impellers | Mechanical Properties | Moderate Strength | |
| Pumps | Corrosion Resistance | Corrosion Resistance | |
| Pumps | Friction & Wear Properties | Wear Resistance | |
| Pumps | Lead Free | Lead-Free Alternative to Leaded Alloy C83600 | |
| Pumps | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Sand Cast | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties