Find suppliers for this alloy C89833
Chemical Composition
Elements
Cu(1) Pb Sn Zn Fe P Ni(2) Al Bi S Sb Si
(1) Cu + Sum of Named Elements 99.3% min.
(2) Ni value includes Co.
Min (%) 86.0 4.0 2.0 1.7
Max (%) 91.0 0.09 6.0 6.0 0.30 0.050 1.0 0.005 2.7 0.08 0.25 0.005
Mechanical Properties *
Form Temper Temper Code Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 500 kg load Izod
(ft-lbs)
* Measured at room temperature, 68°F (20°C).
As Sand Cast As Sand Cast M01 37 Typ
17 Typ
28 Typ
60 Typ
12 Typ
Physical Properties
Melting Point - Liquidus°F 1877
Melting Point - Solidus°F 1454
Densitylb/cu in. at 68°F 0.317
Specific Gravity 8.78
Electrical Conductivity% IACS at 68°F 17.8
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F 41
Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) 13
Specific Heat CapacityBtu/ lb /°F at 68°F 0.085
Modulus of Elasticity in Tensionksi 15500
Casting Characteristics
Casting Attribute Level
Casting Yield High
Drossing Low
Effect of Section Size Low
Fluidity Medium
Gassing Medium
Patternmakers Shrinkage inches per inch 11/64
Shrinkage in Solidification Low
Fabrication Properties
Technique Suitability
Soldering Excellent
Brazing Good
Oxyacetylene Welding Not Recommended
Gas Shielded Arc Welding Not Recommended
Coated Metal Arc Welding Poor
Machinability Rating 81
Common Fabrication Processes

No fabrication process properties for this alloy

Thermal Properties

No thermal properties for this alloy

Typical uses
Product Category Product Reason Category Reason
Industrial Corrosion Resistant, Pressure Tight Castings Corrosion Resistance Corrosion Resistance
Corrosion Resistant, Pressure Tight Castings Friction & Wear Properties Wear Resistance
Corrosion Resistant, Pressure Tight Castings Lead-Free Lead-Free Alternative to Leaded Alloy C83600
Corrosion Resistant, Pressure Tight Castings Mechanical Properties Moderate Strength
Impellers Corrosion Resistance Corrosion Resistance
Impellers Friction & Wear Properties Wear Resistance
Impellers Lead Free Lead-Free Alternative to Leaded Alloy C83600
Impellers Mechanical Properties Moderate Strength
Pumps Corrosion Resistance Corrosion Resistance
Pumps Friction & Wear Properties Wear Resistance
Pumps Lead Free Lead-Free Alternative to Leaded Alloy C83600
Pumps Mechanical Properties Moderate Strength
Applicable Specifications
Form Specific Sub-Form Application System Standard Description
As Sand Cast ASTM B584 COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
Ingot ASTM B30 COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties

No Corrosion Properties Available.