Find suppliers for this alloyC89836
Chemical Composition
Element
Cu(1)PbSnZnFePNi(2)AlBiSSbSi
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co.
Min (%)87.04.02.01.5
Max (%)91.00.257.04.00.350.060.900.0053.50.080.250.005
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 500 kg load
As Sand CastAs Sand CastM0133   Min
37.5   Typ
15   Min
19   Typ
20   Min
30   Typ
65   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1885
Melting Point - Solidus°F1580
Densitylb/cu in. at 68°F0.318
Electrical Conductivity% IACS at 68°F18
Casting Characteristics

No casting characteristics for this alloy

Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingNot Recommended
Coated Metal Arc WeldingPoor
Machinability Rating85
Common Fabrication Processes
  • Casting
Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
PlumbingPlumbing CastingsLead FreeLead Free
Plumbing CastingsMechanical PropertiesModerate Strength
Applicable Specifications
Form System Standard Description
As Sand CastASTMB584COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
IngotASTMB30COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties

No information available.