C89841
| Elements | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Sn | Zn | Fe | Ni(2) | Al | Bi | Mn | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Includes Co. |
||||||||||
| Min (%) | 73.0 | 18.0 | 0.50 | 2.8 | ||||||
| Max (%) | 77.0 | 0.30 | 23.0 | 0.10 | 0.20 | 0.01 | 1.0 | 0.10 | 0.10 | 3.4 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| As Continuous Cast | As Continuous Cast | M07 |
63.1 Typ |
23.5 Typ |
31 Typ |
105 Typ |
| Melting Point - Liquidus°F | 1633 |
|---|---|
| Melting Point - Solidus°F | 1589 |
| Densitylb/cu in. at 68°F | 0.301 |
| Specific Gravity | 8.34 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 22 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 10.3 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Poor |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 85 |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Minimum* | |||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Hot Working Temperature | 1382 | |||
| Stress Relief | 536 | |||
Typical Uses
Applicable Specifications
Corrosion Properties