Find suppliers for this alloy
C89842
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni(2) | Al | Bi | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
|||||||||||
| Min (%) | 78.0 | 2.0 | 0.005 | 0.10 | 1.5 | ||||||
| Max (%) | 82.0 | 0.09 | 3.0 | Rem | 0.30 | 0.02 | 0.50 | 0.005 | 2.5 | 0.05 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| As Continuous Cast | As Continuous Cast | M07 |
35.5 Min 46 Max |
13 Min |
15 Min |
87 Typ |
| Melting Point - Liquidus°F | 1828 |
|---|---|
| Melting Point - Solidus°F | 1591 |
| Densitylb/cu in. at 68°F | 0.31 |
| Specific Gravity | 8.63 |
| Electrical Conductivity% IACS at 68°F | 18.5 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 17.8 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 15.3 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 12.4 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.7 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Minimum* | |||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Stress Relief | 500 | |||
Typical Uses
Applicable Specifications
Corrosion Properties