Find suppliers for this alloy
C89845
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni(2) | Al | Bi | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
|||||||||||
| Min (%) | 82.5 | 3.0 | 6.0 | 1.5 | 1.0 | ||||||
| Max (%) | 87.5 | 0.09 | 5.0 | 9.0 | 0.30 | 0.05 | 2.5 | 0.01 | 2.0 | 0.25 | 0.01 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Fatigue Strength** (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||
| Rod & Bar | As Sand Cast | M01 |
28 Min 32 Typ 38 Max |
15 Min 16 Typ 18 Max |
15 Typ |
67 Typ |
64` Typ |
14 Typ |
| Melting Point - Liquidus°F | 1888 |
|---|---|
| Melting Point - Solidus°F | 1467 |
| Densitylb/cu in. at 68°F | 0.318 |
| Specific Gravity | 8.79 |
| Electrical Conductivity% IACS at 68°F | 14.6 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 36.2 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.7 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.8 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.089 |
| Modulus of Elasticity in Tensionksi | 15700 |
| Modulus of Rigidityksi | 5600 |
| Magnetic Permeability | 0.999 |
| Poisson's Ratio | 0.35 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Medium |
| Effect of Section Size | High |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Medium |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Not Recommended |
| Seam Weld | Not Recommended |
| Butt Weld | Not Recommended |
| Machinability Rating | 76 |
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties