C90800
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.4% min. (2) In determining Cu min., Cu may be calculated as Cu + Ni. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 85.0 | 11.0 | |||||||||
| Max (%) | 89.0 | 0.25 | 13.0 | 0.25 | 0.15 | 0.30 | 0.50 | 0.005 | 0.05 | 0.20 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
50 Min for Standard |
12 Min for Standard |
95 Min for Standard |
| As Sand Cast | As Sand Cast | M01 |
35 Min for Standard |
10 Min for Standard |
65 Min for Standard |
Physical Properties
Casting Characteristics
Fabrication Properties
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Speed Reducers | Corrosion Resistance | Corrosion Resistance |
| Speed Reducers | Friction & Wear Properties | Low Co-efficient of Friction | |
| Speed Reducers | Friction & Wear Properties | Wear Resistance | |
| Speed Reducers | Mechanical Properties | Moderate Strength | |
| Worm Gears | Corrosion Resistance | Corrosion Resistance | |
| Worm Gears | Friction & Wear Properties | Low Co-efficient of Friction | |
| Worm Gears | Friction & Wear Properties | Wear Resistance | |
| Worm Gears | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | ASTM | B427 | GEAR BRONZE ALLOY CASTINGS | |
| As Sand Cast | Castings | ASTM | B427 | GEAR BRONZE ALLOY CASTINGS | |
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties