| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) Cu + Sum of Named Elements 99.3% min. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 86.0 | 1.0 | 5.5 | 3.0 | |||||||
| Max (%) | 90.0 | 2.0 | 6.5 | 5.0 | 0.25 | 0.05 | 1.0 | 0.005 | 0.05 | 0.25 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Charpy V-Notch Impact Strength (ft-lbs) |
Compressive Strength .001 in. set/in. (ksi) |
Compressive Strength .01 in. set/in. (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
Creep Strength (0.1% per 10,000 hours) (ksi) |
Fatigue Strength** (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
34 Min for Standard 34 Min for Standard |
16 Min for Standard |
22 Min for Standard 22 Min for Standard |
|||||||
| As Continuous Cast | As Continuous Cast | M07 |
38 Min for Standard 38 Min for Standard |
19 Min for Standard |
18 Min for Standard 18 Min for Standard |
|||||||
| As Permanent Mold Cast | As Permanent Mold Cast | M05 |
34 Min for Standard |
16 Min for Standard |
24 Min for Standard |
|||||||
| As Sand Cast | As Sand Cast | M01 |
34 Min for Standard 34 Min for Standard 40 Typ |
16 Min for Standard 20 Typ |
22 Min for Standard 22 Min for Standard 30 Typ |
65 Typ |
19 Typ |
15 Typ | 20 Typ | 38 Typ | 11 Typ | 11 Typ |
| Melting Point - Liquidus°F | 1810 |
|---|---|
| Melting Point - Solidus°F | 1518 |
| Densitylb/cu in. at 68°F | 0.312 |
| Specific Gravity | 8.64 |
| Electrical Conductivity% IACS at 68°F | 14 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 40.2 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 14000 |
| Incipient Melting°F | 600 |
| Magnetic Permeability | 1 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Medium |
| Drossing | Low |
| Effect of Section Size | High |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 42 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Architecture | Ornamental Castings | Corrosion Resistance | Corrosion Resistance |
| Ornamental Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Ornamental Castings | Machining Properties | Machinability, Good | |
| Ornamental Castings | Mechanical Properties | Moderate Strength | |
| Building | Cooling Equipment | Conductivity (Thermal) | Thermal Conductivity |
| Cooling Equipment | Corrosion Resistance | Corrosion Resistance | |
| Cooling Equipment | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Cooling Equipment | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
| Cooling Equipment | Machining Properties | Machinability, Good | |
| Cooling Equipment | Mechanical Properties | Moderate Strength | |
| Cooling Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Cooling Equipment | Pressure Tight | Pressure Tight up to 260 C | |
| Heating Equipment | Conductivity (Thermal) | Thermal Conductivity | |
| Heating Equipment | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Heating Equipment | Machining Properties | Machinability, Good | |
| Heating Equipment | Mechanical Properties | Moderate Strength | |
| Heating Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Heating Equipment | Pressure Tight | Pressure Tight up to 260 C | |
| Fasteners | Nuts | Corrosion Resistance | Corrosion Resistance |
| Nuts | Machining Properties | Machinability, Good | |
| Nuts | Mechanical Properties | Moderate Strength | |
| Industrial | Bearings | Corrosion Resistance | Corrosion Resistance |
| Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Machining Properties | Machinability, Good | |
| Bearings | Mechanical Properties | Moderate Strength | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Machining Properties | Machinability, Good | |
| Bushings | Mechanical Properties | Moderate Strength | |
| Cryogenic Valves | Corrosion Resistance | Corrosion Resistance | |
| Cryogenic Valves | Machining Properties | Machinability, Good | |
| Cryogenic Valves | Mechanical Properties | Moderate Strength | |
| Cryogenic Valves | Pressure Tight | Pressure Tight up to 260 C | |
| Fittings Used to 550 F | Corrosion Resistance | Corrosion Resistance | |
| Fittings Used to 550 F | Machining Properties | Machinability, Good | |
| Fittings Used to 550 F | Mechanical Properties | Moderate Strength | |
| Fittings Used to 550 F | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Gears | Corrosion Resistance | Corrosion Resistance | |
| Gears | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Gears | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
| Gears | Friction & Wear Properties | Wear Resistance | |
| Gears | Machining Properties | Machinability, Good | |
| Gears | Mechanical Properties | Moderate Strength | |
| Medium Pressure Hydraulic Equipment | Corrosion Resistance | Corrosion Resistance | |
| Medium Pressure Hydraulic Equipment | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Medium Pressure Hydraulic Equipment | Machining Properties | Machinability, Good | |
| Medium Pressure Hydraulic Equipment | Mechanical Properties | Moderate Strength | |
| Medium Pressure Hydraulic Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Medium Pressure Hydraulic Equipment | Pressure Tight | Pressure Tight up to 260 C | |
| Piston Rings | Corrosion Resistance | Corrosion Resistance | |
| Piston Rings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Piston Rings | Machining Properties | Machinability, Good | |
| Piston Rings | Mechanical Properties | Moderate Strength | |
| Piston Rings | Pressure Tight | Pressure Tight up to 260 C | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pump Impellers | Machining Properties | Machinability, Good | |
| Pump Impellers | Mechanical Properties | Moderate Strength | |
| Pumps Used to 550 F | Corrosion Resistance | Corrosion Resistance | |
| Pumps Used to 550 F | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Pumps Used to 550 F | Corrosion Resistance | Resistant in Saline Solutions | |
| Pumps Used to 550 F | Friction & Wear Properties | Wear Resistance | |
| Pumps Used to 550 F | Machining Properties | Machinability, Good | |
| Pumps Used to 550 F | Mechanical Properties | Moderate Strength | |
| Pumps Used to 550 F | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Valve Components | Corrosion Resistance | Corrosion Resistance | |
| Valve Components | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Valve Components | Corrosion Resistance | Resistant in Saline Solutions | |
| Valve Components | Friction & Wear Properties | Wear Resistance | |
| Valve Components | Machining Properties | Machinability, Good | |
| Valve Components | Mechanical Properties | Moderate Strength | |
| Valves for Water Meters | Corrosion Resistance | Corrosion Resistance | |
| Valves for Water Meters | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Valves for Water Meters | Corrosion Resistance | Resistant in Saline Solutions | |
| Valves for Water Meters | Friction & Wear Properties | Wear Resistance | |
| Valves for Water Meters | Machining Properties | Machinability, Good | |
| Valves for Water Meters | Mechanical Properties | Moderate Strength | |
| Marine | Marine Castings | Corrosion Resistance | Corrosion Resistance |
| Marine Castings | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Marine Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Marine Castings | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
| Marine Castings | Machining Properties | Machinability, Good | |
| Marine Castings | Mechanical Properties | Moderate Strength | |
| Plumbing | Medium Pressure Steam Equipment to 550 F | Corrosion Resistance | Corrosion Resistance |
| Medium Pressure Steam Equipment to 550 F | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Medium Pressure Steam Equipment to 550 F | Machining Properties | Machinability, Good | |
| Medium Pressure Steam Equipment to 550 F | Mechanical Properties | Moderate Strength | |
| Medium Pressure Steam Equipment to 550 F | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Medium Pressure Steam Equipment to 550 F | Pressure Tight | Pressure Tight to 260 C |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| As Continuous Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| As Sand Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Castings | ASTM | B61 | STEAM OR VALVE BRONZE CASTINGS | ||
| Castings | ASME | SB584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Castings | ASME | SB61 | STEAM OR VALVE BRONZE CASTINGS | ||
| Fitting | ASME | SB61 | STEAM OR VALVE BRONZE CASTINGS | ||
| ASTM | B61 | STEAM OR VALVE BRONZE CASTINGS | |||
| FEDERAL | WW-P-460 | PIPE FITTINGS: BRASS OR BRONZE | |||
| ASME | B16.24 | BRONZE PIPE FLANGES AND FLANGED FITTINGS | |||
| Flanges | ASTM | B61 | STEAM OR VALVE BRONZE CASTINGS | ||
| ASME | SB61 | STEAM OR VALVE BRONZE CASTINGS | |||
| FEDERAL | WW-P-460 | PIPE FITTINGS: BRASS OR BRONZE | |||
| Ingot | |||||
| ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | |||
| Valves | |||||
| MILITARY | MIL-V-17547 | VALVE, CHECK, BRONZE |
Corrosion Properties