SSL certificate problem: certificate has expired
Find suppliers for this alloy C92300
Chemical Composition
Elements
Cu(1,2) Pb Sn Zn Fe P(3) Ni(4) Al S Sb Si
(1) Cu + Sum of Named Elements 99.3% min.
(2) In determining Cu min., Cu may be calculated as Cu + Ni.
(3) For continuous castings P shall be 1.5% max.
(4) Ni value includes Co.
Min (%) 85.0 0.30 7.5 2.5
Max (%) 89.0 1.0 9.0 5.0 0.25 0.05 1.0 0.005 0.05 0.25 0.005
Mechanical Properties *
Form Temper Temper Code Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 500 kg load Izod
(ft-lbs)
Compressive Strength .001 in. set/in.
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
* Measured at room temperature, 68°F (20°C).
As Centrifugal Cast As Centrifugal Cast M02 36 Min for Standard
36 Min for Standard
16 Min for Standard
18 Min for Standard
18 Min for Standard
As Continuous Cast As Continuous Cast M07 40 Min for Standard
40 Min for Standard
19 Min for Standard
16 Min for Standard
16 Min for Standard
As Sand Cast As Sand Cast M01 36 Min for Standard
36 Min for Standard
40 Typ
16 Min for Standard
20 Typ
18 Min for Standard
18 Min for Standard
25 Typ
70 Typ
12 Typ 10 Typ 35 Typ
Physical Properties
Melting Point - Liquidus°F 1830
Melting Point - Solidus°F 1570
Densitylb/cu in. at 68°F 0.317
Specific Gravity 8.77
Electrical Conductivity% IACS at 68°F 12
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F 43.2
Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) 10
Specific Heat CapacityBtu/ lb /°F at 68°F 0.09
Modulus of Elasticity in Tensionksi 14000
Incipient Melting°F 600
Casting Characteristics
Casting Attribute Level
Casting Yield Medium
Drossing Low
Effect of Section Size High
Fluidity Medium
Gassing Medium
Patternmakers Shrinkage inches per inch 3/16
Shrinkage in Solidification Low
Fabrication Properties
Technique Suitability
Soldering Excellent
Brazing Good
Oxyacetylene Welding Not Recommended
Gas Shielded Arc Welding Not Recommended
Coated Metal Arc Welding Not Recommended
Machinability Rating 42
Common Fabrication Processes

No fabrication process properties for this alloy

Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief 500
Solution Treatment 0
Typical uses
Product Category Product Reason Category Reason
Builders Hardware Structural Castings Corrosion Resistance Corrosion Resistance
Structural Castings Corrosion Resistance Corrosion Resistance to Numerous Environments
Structural Castings Machining Properties Machinability, Good
Structural Castings Mechanical Properties Moderate Strength
Fasteners Nuts Corrosion Resistance Corrosion Resistance
Nuts Corrosion Resistance Corrosion Resistance to Fresh Water
Nuts Corrosion Resistance Corrosion Resistance to Numerous Environments
Nuts Corrosion Resistance Corrosion Resistance to Saline Solutions
Nuts Machining Properties Machinability, Good
Nuts Mechanical Properties Moderate Strength
Industrial Bearings Corrosion Resistance Corrosion Resistance
Bearings Corrosion Resistance Corrosion Resistance to Numerous Environments
Bearings Friction & Wear Properties Wear Resistance
Bearings Machining Properties Machinability, Good
Bearings Mechanical Properties Moderate Strength
Bushings Corrosion Resistance Corrosion Resistance
Bushings Friction & Wear Properties Wear Resistance
Bushings Machining Properties Machinability, Good
Bushings Mechanical Properties Moderate Strength
Gears Corrosion Resistance Corrosion Resistance
Gears Friction & Wear Properties Wear Resistance
Gears Machining Properties Machinability, Good
Gears Mechanical Properties Moderate Strength
High Pressure Hydraulic Equipment Corrosion Resistance Corrosion Resistance
High Pressure Hydraulic Equipment Corrosion Resistance Corrosion Resistance to Fresh Water
High Pressure Hydraulic Equipment Corrosion Resistance Corrosion Resistance to Numerous Environments
High Pressure Hydraulic Equipment Corrosion Resistance Corrosion Resistance to Saline Solutions
High Pressure Hydraulic Equipment Friction & Wear Properties Wear Resistance
High Pressure Hydraulic Equipment Machining Properties Machinability, Good
High Pressure Hydraulic Equipment Mechanical Properties Moderate Strength
High Pressure Hydraulic Equipment Pressure Tight Pressure Tight below 260 C
Piston Rings Corrosion Resistance Corrosion Resistance
Piston Rings Corrosion Resistance Corrosion Resistance to Numerous Environments
Piston Rings Machining Properties Machinability, Good
Piston Rings Mechanical Properties Moderate Strength
Piston Rings Pressure Tight Pressure Tight below 260 C
Pump Impellers Corrosion Resistance Corrosion Resistance
Pump Impellers Corrosion Resistance Corrosion Resistance to Fresh Water
Pump Impellers Corrosion Resistance Corrosion Resistance to Saline Solutions
Pump Impellers Friction & Wear Properties Wear Resistance
Pump Impellers Machining Properties Machinability, Good
Pump Impellers Mechanical Properties Moderate Strength
Pump Parts Corrosion Resistance Corrosion Resistance
Pump Parts Corrosion Resistance Corrosion Resistance to Fresh Water
Pump Parts Corrosion Resistance Corrosion Resistance to Numerous Environments
Pump Parts Corrosion Resistance Corrosion Resistance to Saline Solutions
Pump Parts Friction & Wear Properties Wear Resistance
Pump Parts Machining Properties Machinability, Good
Pump Parts Mechanical Properties Moderate Strength
Valve Bodies Corrosion Resistance Corrosion Resistance
Valve Bodies Corrosion Resistance Corrosion Resistance to Fresh Water
Valve Bodies Corrosion Resistance Corrosion Resistance to Saline Solutions
Valve Bodies Machining Properties Machinability, Good
Valve Bodies Mechanical Properties Moderate Strength
Plumbing High Pressure Steam Equipment Corrosion Resistance Corrosion Resistance
High Pressure Steam Equipment Corrosion Resistance Corrosion Resistance to Fresh Water
High Pressure Steam Equipment Corrosion Resistance Corrosion Resistance to Numerous Environments
High Pressure Steam Equipment Corrosion Resistance Corrosion Resistance to Saline Solutions
High Pressure Steam Equipment Machining Properties Machinability, Good
High Pressure Steam Equipment Mechanical Properties Moderate Strength
High Pressure Steam Equipment Pressure Tight Pressure Tight below 260 C
Applicable Specifications
Form Specific Sub-Form Application System Standard Description
As Centrifugal Cast Castings SAE J462 CAST COPPER ALLOYS
Castings ASTM B271/B271M COPPER BASE ALLOY CENTRIFUGAL CASTINGS
Castings SAE J461 WROUGHT AND CAST COPPER ALLOYS
As Continuous Cast Castings SAE J462 CAST COPPER ALLOYS
Castings ASTM B505/B505M COPPER BASE ALLOY CONTINUOUS CASTINGS
Castings SAE J461 WROUGHT AND CAST COPPER ALLOYS
As Sand Cast Castings SAE J461 WROUGHT AND CAST COPPER ALLOYS
Castings ASTM B584 COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
Castings ASTM B763/B763M COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
Ingot
ASTM B30 COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties

No Corrosion Properties Available.