C92500
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.3% min. (2) In determining Cu min., Cu may be calculated as Cu + Ni. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 85.0 | 1.0 | 10.0 | 0.8 | |||||||
| Max (%) | 88.0 | 1.5 | 12.0 | 0.50 | 0.30 | 0.30 | 1.5 | 0.005 | 0.05 | 0.25 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| As Continuous Cast | As Continuous Cast | M07 |
40 Min for Standard 40 Min for Standard |
24 Min for Standard |
10 Min for Standard 10 Min for Standard |
|
| As Sand Cast | As Sand Cast | M01 |
35 Min for Standard 44 Typ |
20 Typ |
10 Min for Standard 20 Typ |
80 Typ |
| Densitylb/cu in. at 68°F | 0.317 |
|---|---|
| Specific Gravity | 8.7 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 16000 |
| Incipient Melting°F | 600 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Medium |
| Drossing | Low |
| Effect of Section Size | High |
| Fluidity | High |
| Gassing | Med-High |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 30 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Automotive Synchronizer Rings | Corrosion Resistance | Corrosion Resistance |
| Automotive Synchronizer Rings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Automotive Synchronizer Rings | Friction & Wear Properties | Wear Resistance | |
| Automotive Synchronizer Rings | Mechanical Properties | Moderate Strength | |
| Industrial | Gears | Corrosion Resistance | Corrosion Resistance |
| Gears | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Gears | Friction & Wear Properties | Wear Resistance | |
| Gears | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Continuous Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| As Sand Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
| Valves |
Corrosion Properties