Chemical Composition
Element
Cu(1)PbSnZnFeP(2)Ni(3)AlSSbSi
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) For continuous castings P shall be 1.5% max. (3) Ni value includes Co. Cu + Sum of Named Elements 99.3% min.
Min (%)86.00.89.31.3
Max (%)88.51.510.52.50.200.030.70.0050.050.250.005
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell F scale
Brinell Hardness, 500 kg load
Izod
(ft-lbs)
Compressive Strength .001 in. set/in.
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
As Sand CastAs Sand CastM0140   Min for Standard
44   Typ
18   Min for Standard
20   Typ
20   Min for Standard
30   Typ
78   Typ
70   Typ
7   Typ
12   Typ
40   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1800
Melting Point - Solidus°F1550
Densitylb/cu in. at 68°F0.315
Specific Gravity8.72
Electrical Conductivity% IACS at 68°F9
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)10
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Casting Characteristics
Casting Attribute Level
Casting YieldMedium
DrossingLow
Effect of Section SizeHigh
FluidityMedium
GassingMedium
Patternmakers Shrinkageinches per inch3/16
Shrinkage in SolidificationLow
Fabrication Properties
Technique Suitability Footnote
SolderingExcellent
BrazingGoodSince brazing is performed in the hot short temperature range, strain must be avoided during brazing and cooling.
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingNot Recommended
Coated Metal Arc WeldingNot Recommended
Machinability Rating40
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief500
Solution Treatment0
Typical uses
Product Category Product Reason Category Reason
FastenersLead Screw NutsCorrosion ResistanceCorrosion Resistance
Lead Screw NutsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Lead Screw NutsMachining PropertiesMachinability, Good
Lead Screw NutsMechanical PropertiesModerate Strength
NutsCorrosion ResistanceCorrosion Resistance
NutsCorrosion ResistanceCorrosion Resistance to Numerous Environments
NutsMachining PropertiesMachinability, Good
NutsMechanical PropertiesModerate Strength
IndustrialBushingsCorrosion ResistanceCorrosion Resistance
BushingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
BushingsFriction & Wear PropertiesWear Resistance
BushingsMachining PropertiesMachinability, Good
BushingsMechanical PropertiesModerate Strength
FittingsCorrosion ResistanceCorrosion Resistance
FittingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
FittingsMachining PropertiesMachinability, Good
FittingsMechanical PropertiesModerate Strength
GearsCorrosion ResistanceCorrosion Resistance
GearsCorrosion ResistanceCorrosion Resistance to Fresh Water
GearsCorrosion ResistanceCorrosion Resistance to Numerous Environments
GearsCorrosion ResistanceCorrosion Resistance to Saline Solutions
GearsMachining PropertiesMachinability, Good
GearsMechanical PropertiesModerate Strength
Heavy Duty BearingsCorrosion ResistanceCorrosion Resistance
Heavy Duty BearingsCorrosion ResistanceCorrosion Resistance to Fresh Water
Heavy Duty BearingsCorrosion ResistanceCorrosion Resistance to Saline Solutions
Heavy Duty BearingsFriction & Wear PropertiesWear Resistance
Heavy Duty BearingsMachining PropertiesMachinability, Good
Heavy Duty BearingsMechanical PropertiesModerate Strength
Piston RingsCorrosion ResistanceCorrosion Resistance
Piston RingsCorrosion ResistanceCorrosion Resistance to Fresh Water
Piston RingsCorrosion ResistanceCorrosion Resistance to Saline Solutions
Piston RingsFriction & Wear PropertiesWear Resistance
Piston RingsMachining PropertiesMachinability, Good
Piston RingsMechanical PropertiesModerate Strength
Piston RingsPressure TightPressure Tight below 260 C
Pump ImpellersCorrosion ResistanceCorrosion Resistance
Pump ImpellersCorrosion ResistanceCorrosion Resistance to Fresh Water
Pump ImpellersCorrosion ResistanceCorrosion Resistance to Numerous Environments
Pump ImpellersCorrosion ResistanceCorrosion Resistance to Saline Solutions
Pump ImpellersFriction & Wear PropertiesWear Resistance
Pump ImpellersMachining PropertiesMachinability, Good
Pump ImpellersMechanical PropertiesModerate Strength
Pump PistonsCorrosion ResistanceCorrosion Resistance
Pump PistonsCorrosion ResistanceCorrosion Resistance to Fresh Water
Pump PistonsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Pump PistonsCorrosion ResistanceCorrosion Resistance to Saline Solutions
Pump PistonsFriction & Wear PropertiesWear Resistance
Pump PistonsMachining PropertiesMachinability, Good
Pump PistonsMechanical PropertiesModerate Strength
Steam CastingsCorrosion ResistanceCorrosion Resistance
Steam CastingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Steam CastingsFriction & Wear PropertiesWear Resistance
Steam CastingsMachining PropertiesMachinability, Good
Steam CastingsMechanical PropertiesModerate Strength
Steam CastingsPressure TightPressure Tight below 260 C
Valve BodiesCorrosion ResistanceCorrosion Resistance
Valve BodiesCorrosion ResistanceCorrosion Resistance to Fresh Water
Valve BodiesCorrosion ResistanceCorrosion Resistance to Numerous Environments
Valve BodiesCorrosion ResistanceCorrosion Resistance to Saline Solutions
Valve BodiesMachining PropertiesMachinability, Good
Valve BodiesMechanical PropertiesModerate Strength
ValvesCorrosion ResistanceCorrosion Resistance
ValvesCorrosion ResistanceCorrosion Resistance to Fresh Water
ValvesCorrosion ResistanceCorrosion Resistance to Numerous Environments
ValvesCorrosion ResistanceCorrosion Resistance to Saline Solutions
ValvesFriction & Wear PropertiesWear Resistance
ValvesMachining PropertiesMachinability, Good
ValvesMechanical PropertiesModerate Strength
Applicable Specifications
Form Sub-Form System Standard Description
As Sand CastCastingsASTMB584COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
ValvesASTMB763/B763MCOPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
Ingot
ASTMB30COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties

No information available.