Find suppliers for this alloy
C93200
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.0% min. (2) In determining Cu min., Cu may be calculated as Cu + Ni. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 81.0 | 6.0 | 6.3 | 1.0 | |||||||
| Max (%) | 85.0 | 8.0 | 7.5 | 4.0 | 0.20 | 0.15 | 1.0 | 0.005 | 0.08 | 0.35 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Izod (ft-lbs) |
Compressive Strength .1 in. set/in. (ksi) |
Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
30 Min for Standard |
14 Min for Standard |
15 Min for Standard |
|||||
| As Continuous Cast | As Continuous Cast | M07 |
35 Min for Standard 35 Min for Standard |
20 Min for Standard |
10 Min for Standard 10 Min for Standard |
|||||
| As Sand Cast | As Sand Cast | M01 |
30 Min for Standard 30 Min for Standard 35 Typ |
14 Min for Standard 18 Typ |
15 Min for Standard 15 Min for Standard 20 Typ |
65 Typ |
6 Typ | 46 Typ | 16 Typ | 8.5 Typ |
| Melting Point - Liquidus°F | 1790 |
|---|---|
| Melting Point - Solidus°F | 1570 |
| Densitylb/cu in. at 68°F | 0.322 |
| Specific Gravity | 8.91 |
| Electrical Conductivity% IACS at 68°F | 12 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 33.6 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 14500 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | Medium |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 7/32 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 70 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Automotive Fittings | Corrosion Resistance | Corrosion Resistance |
| Automotive Fittings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Automotive Fittings | Machining Properties | Machinability, Good | |
| Automotive Fittings | Mechanical Properties | Relatively Low Strength | |
| Fasteners | Washers | Corrosion Resistance | Corrosion Resistance |
| Washers | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Washers | Machining Properties | Machinability, Good | |
| Washers | Mechanical Properties | Relatively Low Strength | |
| Industrial | Bearings | Corrosion Resistance | Corrosion Resistance |
| Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Machining Properties | Machinability, Good | |
| Bearings | Mechanical Properties | Relatively Low Strength | |
| Bearings for Cranes | Corrosion Resistance | Corrosion Resistance | |
| Bearings for Cranes | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings for Cranes | Friction & Wear Properties | Anti-Seizing Properties | |
| Bearings for Cranes | Friction & Wear Properties | Low Coefficient of Friction | |
| Bearings for Cranes | Friction & Wear Properties | Wear Resistance | |
| Bearings for Cranes | Machining Properties | Machinability, Good | |
| Bearings for Cranes | Mechanical Properties | Relatively Low Strength | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Machining Properties | Machinability, Good | |
| Bushings | Mechanical Properties | Relatively Low Strength | |
| Diesel Engine Wrist Pin Bushings | Corrosion Resistance | Corrosion Resistance | |
| Diesel Engine Wrist Pin Bushings | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Diesel Engine Wrist Pin Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Diesel Engine Wrist Pin Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| Diesel Engine Wrist Pin Bushings | Friction & Wear Properties | Wear Resistance | |
| Diesel Engine Wrist Pin Bushings | Machining Properties | Machinability, Good | |
| Diesel Engine Wrist Pin Bushings | Mechanical Properties | Relatively Low Strength | |
| Fittings | Corrosion Resistance | Corrosion Resistance | |
| Fittings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Fittings | Machining Properties | Machinability, Good | |
| Fittings | Mechanical Properties | Relatively Low Strength | |
| Forging Press Toggle Lever Bearings | Corrosion Resistance | Corrosion Resistance | |
| Forging Press Toggle Lever Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Forging Press Toggle Lever Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Forging Press Toggle Lever Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Forging Press Toggle Lever Bearings | Friction & Wear Properties | Wear Resistance | |
| Forging Press Toggle Lever Bearings | Machining Properties | Machinability, Good | |
| Forging Press Toggle Lever Bearings | Mechanical Properties | Relatively Low Strength | |
| Fuel Pump Bushings | Corrosion Resistance | Corrosion Resistance | |
| Fuel Pump Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Fuel Pump Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Fuel Pump Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| Fuel Pump Bushings | Friction & Wear Properties | Wear Resistance | |
| Fuel Pump Bushings | Machining Properties | Machinability, Good | |
| Fuel Pump Bushings | Mechanical Properties | Relatively Low Strength | |
| General Purpose Bushings | Corrosion Resistance | Corrosion Resistance | |
| General Purpose Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| General Purpose Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| General Purpose Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| General Purpose Bushings | Friction & Wear Properties | Wear Resistance | |
| General Purpose Bushings | Machining Properties | Machinability, Good | |
| General Purpose Bushings | Mechanical Properties | Relatively Low Strength | |
| Hydraulic Press Main Lining | Corrosion Resistance | Corrosion Resistance | |
| Hydraulic Press Main Lining | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Hydraulic Press Main Lining | Friction & Wear Properties | Anti-Seizing Properties | |
| Hydraulic Press Main Lining | Friction & Wear Properties | Wear Resistance | |
| Hydraulic Press Main Lining | Machining Properties | Machinability, Good | |
| Hydraulic Press Main Lining | Mechanical Properties | Relatively Low Strength | |
| Hydraulic Press Stuffing Box | Corrosion Resistance | Corrosion Resistance | |
| Hydraulic Press Stuffing Box | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Hydraulic Press Stuffing Box | Machining Properties | Machinability, Good | |
| Hydraulic Press Stuffing Box | Mechanical Properties | Relatively Low Strength | |
| Hydraulic Press Stuffing Box | Pressure Tight | Pressure Tight | |
| Insert Bearings | Corrosion Resistance | Corrosion Resistance | |
| Insert Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Insert Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Insert Bearings | Friction & Wear Properties | Wear Resistance | |
| Insert Bearings | Machining Properties | Machinability, Good | |
| Insert Bearings | Mechanical Properties | Relatively Low Strength | |
| Linkage Bushings for Presses | Corrosion Resistance | Corrosion Resistance | |
| Linkage Bushings for Presses | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Linkage Bushings for Presses | Friction & Wear Properties | Anti-Seizing Properties | |
| Linkage Bushings for Presses | Friction & Wear Properties | Low Coefficient of Friction | |
| Linkage Bushings for Presses | Friction & Wear Properties | Wear Resistance | |
| Linkage Bushings for Presses | Machining Properties | Machinability, Good | |
| Linkage Bushings for Presses | Mechanical Properties | Relatively Low Strength | |
| Machine Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Machine Parts | Friction & Wear Properties | Anti-Seizing Properties | |
| Machine Parts | Friction & Wear Properties | Wear Resistance | |
| Machine Parts | Machining Properties | Machinability, Good | |
| Machine Parts | Mechanical Properties | Relatively Low Strength | |
| Machine Tool Bearings | Corrosion Resistance | Corrosion Resistance | |
| Machine Tool Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Machine Tool Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Machine Tool Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Machine Tool Bearings | Friction & Wear Properties | Wear Resistance | |
| Machine Tool Bearings | Machining Properties | Machinability, Good | |
| Machine Tool Bearings | Mechanical Properties | Relatively Low Strength | |
| Main Spindle Bearings | Corrosion Resistance | Corrosion Resistance | |
| Main Spindle Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Main Spindle Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Main Spindle Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Main Spindle Bearings | Friction & Wear Properties | Wear Resistance | |
| Main Spindle Bearings | Machining Properties | Machinability, Good | |
| Main Spindle Bearings | Mechanical Properties | Relatively Low Strength | |
| Pump Fixtures | Corrosion Resistance | Corrosion Resistance | |
| Pump Fixtures | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pump Fixtures | Machining Properties | Machinability, Good | |
| Pump Fixtures | Mechanical Properties | Relatively Low Strength | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Petroleum Products | |
| Pump Impellers | Friction & Wear Properties | Wear Resistance | |
| Pump Impellers | Machining Properties | Machinability, Good | |
| Pump Impellers | Mechanical Properties | Relatively Low Strength | |
| Pumps | Corrosion Resistance | Corrosion Resistance | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pumps | Friction & Wear Properties | Wear Resistance | |
| Pumps | Machining Properties | Machinability, Good | |
| Pumps | Mechanical Properties | Relatively Low Strength | |
| Pumps | Pressure Tight | Pressure Tight | |
| Roll Neck Bearings | Corrosion Resistance | Corrosion Resistance | |
| Roll Neck Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Roll Neck Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Roll Neck Bearings | Friction & Wear Properties | Wear Resistance | |
| Roll Neck Bearings | Machining Properties | Machinability, Good | |
| Roll Neck Bearings | Mechanical Properties | Relatively Low Strength | |
| Rolling Mill Bearings | Corrosion Resistance | Corrosion Resistance | |
| Rolling Mill Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Rolling Mill Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Rolling Mill Bearings | Friction & Wear Properties | Wear Resistance | |
| Rolling Mill Bearings | Machining Properties | Machinability, Good | |
| Rolling Mill Bearings | Mechanical Properties | Relatively Low Strength | |
| Thrust Washers | Corrosion Resistance | Corrosion Resistance | |
| Thrust Washers | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Thrust Washers | Friction & Wear Properties | Wear Resistance | |
| Thrust Washers | Machining Properties | Machinability, Good | |
| Thrust Washers | Mechanical Properties | Relatively Low Strength | |
| Trunion Bearings | Corrosion Resistance | Corrosion Resistance | |
| Trunion Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Trunion Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Trunion Bearings | Friction & Wear Properties | Wear Resistance | |
| Trunion Bearings | Machining Properties | Machinability, Good | |
| Trunion Bearings | Mechanical Properties | Relatively Low Strength | |
| Water Pump Bushings | Corrosion Resistance | Corrosion Resistance | |
| Water Pump Bushings | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Water Pump Bushings | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Water Pump Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Water Pump Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| Water Pump Bushings | Friction & Wear Properties | Wear Resistance | |
| Water Pump Bushings | Machining Properties | Machinability, Good | |
| Water Pump Bushings | Mechanical Properties | Relatively Low Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | ||
| As Continuous Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| As Permanent Mold Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| As Sand Cast | Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | |
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| ASTM | B66 | BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS | |||
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
Corrosion Properties